Desulfurization adsorbents, methods of making and using the same

By preparing a desulfurization adsorbent composed of zinc-aluminum hydrotalcite with a layered structure and zinc oxide, the problems of low sulfur capacity and low utilization rate of active components in zinc oxide-based room temperature desulfurizers were solved, achieving efficient room temperature desulfurization and simple industrial application.

CN117917259BActive Publication Date: 2026-11-24CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211288726.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-20
Publication Date
2026-11-24
Estimated Expiration
2042-10-20

AI Technical Summary

Technical Problem

Existing zinc oxide-based room-temperature desulfurization adsorbents have low sulfur capacity, low utilization of active components, and complex preparation processes.

Method used

A desulfurization adsorbent composed of zinc-aluminum hydrotalcite and zinc oxide was prepared by co-precipitation technology. Through co-flow co-precipitation and calcination, zinc-aluminum hydrotalcite with a layered structure was formed, which improved the dispersibility of zinc oxide and the utilization rate of active components.

Benefits of technology

It achieves improved sulfur capacity and utilization rate of active components, and is particularly suitable for desulfurization at room temperature. The process is simple and easy to control, making it suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117917259B_ABST
    Figure CN117917259B_ABST
Patent Text Reader

Abstract

The present application relates to raw material purification technical field, specifically to a kind of desulfurization adsorbent and its preparation method and application.The desulfurization adsorbent contains: A) 15-30 parts zinc-aluminum hydrotalcite;B) 50-90 parts zinc oxide;C) 1-15 parts alumina, by weight.The structural formula of the zinc-aluminum hydrotalcite is Zn 1‑x Al x (OH)2(CO3) x / 2 ·nH2O, wherein x is 0.30-0.44, n is an integer of 3-6.The desulfurization adsorbent is used for H2S-containing material desulfurization, which is beneficial to the diffusion of H2S, so that the desulfurization adsorbent has greater sulfur capacity and active component utilization rate, and is particularly suitable for normal temperature desulfurization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of raw material purification technology, specifically to a desulfurization adsorbent, its preparation method, and its application. Background Technology

[0002] Hydrogen feedstocks derived from natural gas, syngas, coke oven gas, and fossil fuels typically contain H2S impurities. The presence of H2S corrodes equipment and pollutes the environment. Furthermore, hydrogen sulfide present in the feedstock can poison downstream catalysts. For example, H2S in syngas can poison methanol catalysts using copper, zinc, and aluminum as active components, and trace amounts of H2S in hydrogen feedstocks can poison fuel cell catalysts. Therefore, industrial plants impose strict requirements on the H2S impurity content of feedstocks. In the syngas-to-methanol process, the sulfur content in the syngas must be less than 1 ppm, and for hydrogen used in fuel cells, the sulfur content must be less than 4 ppb. Therefore, feedstocks must be purified to remove H2S impurities before entering the main reaction unit. Zinc oxide is a highly effective desulfurization adsorbent for deep H2S removal. It reacts with H2S to form ZnS, which is difficult to dissociate, offering advantages such as high desulfurization precision, ease of use, reliability, and high sulfur capacity. It plays a crucial role in "gatekeeping" and "protection" in chemical processes. Improving the low-temperature sulfur capacity of zinc oxide-based desulfurizers is a key focus of desulfurization technology research.

[0003] CN102512942A discloses a low-temperature fine desulfurizing agent and its preparation method. The raw materials for preparing the fine desulfurizing agent include 40-60% basic zinc carbonate, 15-25% copper carbonate, and at least one of the following: 0-10% pore-forming agent, 0-10% binder, and 5-10% extrusion aid. It is characterized by including 20-30% waste agent to enhance catalyst strength and simplify the preparation process. Furthermore, the raw materials include 0-10% lubricant to improve the binding between materials. After the above substances are mixed evenly, 5-10% extrusion aid is added. After kneading and molding, the mixture is dried at 100-120℃ for 3-4 hours to obtain a fine desulfurizing agent that can be used at low temperatures. It is suitable for fine desulfurization of industrial gases such as natural gas, associated gas from petroleum gas, refinery waste gas, and coal gas. Although this desulfurizing agent has a high sulfur capacity, the operating temperature still needs to be above 100℃.

[0004] CN101337150A discloses a method for preparing a mesoporous desulfurizer containing nano-zinc oxide. The method uses a mesoporous material as the desulfurizer carrier and nano-sized zinc oxide particles as the desulfurization catalyst. The nano-sized zinc oxide particles are loaded onto the mesoporous material to obtain a zinc oxide-containing mesoporous desulfurizer. Physical characterization and desulfurization performance testing of the synthesized desulfurizer show that the zinc oxide nanoparticles are well dispersed and mainly deposited within mesopores and micropores. Furthermore, the desulfurizer exhibits excellent H2S removal capacity at room temperature. Moreover, the sulfur penetration capacity of the mesoporous desulfurizer increases with increasing nano-zinc oxide content. However, the microwave synthesis process used in the preparation of this desulfurizer makes large-scale application difficult.

[0005] CN104307318A discloses a method for preparing a zinc oxide room-temperature desulfurizing agent. The method involves first forming unstable precipitates from a portion of zinc and copper salts, and then completely converting the remaining unprecipitated zinc and copper salts, along with the unstable precipitates, into stable hydroxide and copper hydroxide precipitates in a double-cone rotary vacuum reactor. The resulting composite powder of zinc oxide and copper oxide is then calcined to obtain the zinc oxide room-temperature desulfurizing agent. This desulfurizing agent incorporates copper additives and utilizes a vacuum reactor, resulting in high production costs. Summary of the Invention

[0006] The purpose of this invention is to overcome the problems of low sulfur capacity, low utilization of active components, and complex preparation process of existing zinc oxide-based room temperature desulfurization adsorbents, and to provide a room temperature desulfurization adsorbent with high sulfur capacity and high utilization of active components.

[0007] To achieve the above objectives, a first aspect of the present invention provides a desulfurization adsorbent, comprising, by weight: A) 15-30 parts of zinc-aluminum hydrotalcite; B) 50-90 parts of zinc oxide; and C) 1-15 parts of aluminum oxide; wherein the zinc-aluminum hydrotalcite has the structural formula Zn 1-x Al x (OH)2(CO3) x / 2 ·nH2O, where x is 0.30 to 0.44 and n is an integer from 3 to 6.

[0008] A second aspect of the present invention provides a method for preparing the desulfurization adsorbent of the present invention, the method comprising:

[0009] (1) The zinc-aluminum hydrotalcite is obtained by first co-precipitation of zinc-aluminum solution a and alkaline solution b, followed by separation and drying; in alkaline solution b, the alkaline substance is selected from at least one of alkaline carbonate or bicarbonate; in solution a, the molar ratio of Zn:Al is 7:3 to 3:7.

[0010] (2) The solution containing zinc and aluminum, c, and the alkaline solution, d, were subjected to a second co-precipitation to obtain a mixed solution. The solution was then filtered, dried, and calcined to obtain a component containing zinc oxide and aluminum oxide.

[0011] (3) Zinc-aluminum hydrotalcite and components containing zinc oxide and aluminum oxide are mixed and molded to obtain a desulfurization adsorbent.

[0012] A third aspect of the present invention provides the application of the desulfurization adsorbent described herein in the desulfurization of H2S-containing materials.

[0013] Through the above technical solution, the layered structure of the zinc-aluminum hydrotalcite in the desulfurization adsorbent provided by the present invention is conducive to the further dispersion of the active component (zinc oxide); the desulfurization adsorbent is used for desulfurization of H2S-containing materials, which is conducive to the diffusion of H2S, and therefore the desulfurization adsorbent has a larger sulfur capacity and active component utilization rate, and is particularly suitable for desulfurization at room temperature; preferably, when the zinc oxide grain size is less than 12nm, the dispersibility of zinc oxide can be further improved, and the sulfur capacity and active component utilization rate of the desulfurization adsorbent can be improved.

[0014] This invention uses co-precipitation technology to prepare active components. The process is simple and easy to control, which is beneficial for large-scale industrial applications. Attached Figure Description

[0015] Figure 1 This is the XRD pattern of the desulfurization adsorbent prepared in Example 1. Detailed Implementation

[0016] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0017] In this invention, I(003) / I(100) refers to the ratio of the intensity of the (003) crystal plane diffraction peak to the intensity of the (100) crystal plane diffraction peak in the XRD pattern of the desulfurization adsorbent.

[0018] The first aspect of this invention provides a desulfurization adsorbent, comprising, by weight: A) 15-30 parts of zinc-aluminum hydrotalcite; B) 50-90 parts of zinc oxide; C) 1-15 parts of aluminum oxide; wherein the zinc-aluminum hydrotalcite has the structural formula Zn 1-x Al x (OH)2(CO3) x / 2 ·nH2O, where x is 0.30 to 0.44 and n is an integer from 3 to 6.

[0019] According to a preferred embodiment of the present invention, the I(003) / I(100) ratio in the XRD pattern of the desulfurization adsorbent is 5.6 to 6.8.

[0020] According to a preferred embodiment of the present invention, the specific surface area of ​​the desulfurization adsorbent is 150-200 m². 2 / g, pore volume greater than 0.3-0.5cm 3 / g.

[0021] In this invention, the particle size of the zinc oxide can be selected over a wide range. According to a preferred embodiment of the invention, the particle size of the zinc oxide crystals is not higher than 12 nm, preferably 8 to 11 nm; within this particle size range, it is beneficial to further improve the dispersibility of zinc oxide.

[0022] According to a preferred embodiment of the present invention, the content of zinc-aluminum hydrotalcite is 18-25 parts by weight, the content of zinc oxide is 55-85 parts by weight, and the content of aluminum oxide is 2-13 parts by weight; this is beneficial to further improve the dispersibility of zinc oxide and improve the sulfur capacity and utilization rate of the active components of the desulfurization adsorbent.

[0023] All desulfurization adsorbents possessing the aforementioned properties can achieve the objectives of this invention. This invention does not impose particular requirements on the preparation method of the desulfurization adsorbent. According to a preferred embodiment of this invention, this invention provides a method for preparing the desulfurization adsorbent described herein, the method comprising:

[0024] (1) The zinc-aluminum hydrotalcite is obtained by first co-precipitation of zinc-aluminum solution a and alkaline solution b, followed by separation and drying; in solution a, the molar ratio of Zn:Al is 7:3 to 3:7; in the alkaline solution b, the alkaline substance is selected from at least one of alkaline carbonate or bicarbonate.

[0025] (2) The solution containing zinc and aluminum, c, and the alkaline solution, d, were subjected to a second co-precipitation to obtain a mixed solution. The solution was then filtered, dried, and calcined to obtain a component containing zinc oxide and aluminum oxide.

[0026] (3) Zinc-aluminum hydrotalcite and components containing zinc oxide and aluminum oxide are mixed and molded to obtain a desulfurization adsorbent.

[0027] In this invention, steps (1) and (2) are distinguished only by their different steps, and the order of steps (1) and (2) is not limited.

[0028] According to a preferred embodiment of the present invention, in step (1), the first coprecipitation conditions include: pH 8 to 12, preferably 9 to 11; temperature 40 to 90°C; and time 0.5 to 3 hours.

[0029] In this invention, the concentrations of zinc and aluminum in solution a can be selected within a wide range. According to a preferred embodiment of this invention, the molar concentration of Zn in solution a is 0.1 to 1.0 mol / L, and the molar concentration of Al is 0.1 to 1.0 mol / L.

[0030] In this invention, the concentration of alkaline substance in alkaline solution b can be selected from a wide range. According to a preferred embodiment of this invention, the molar concentration of alkaline substance in alkaline solution b is 1.5 to 2.0 mol / L.

[0031] According to a preferred embodiment of the present invention, step (2), the second coprecipitation conditions include: pH 5 to 9, preferably 6 to 8; temperature 40 to 90°C; and time 0.5 to 3 hours.

[0032] In this invention, the concentrations of zinc and aluminum in solution c can be selected within a wide range. According to a preferred embodiment of this invention, in solution c, the molar ratio of Zn:Al is 10:1 to 4:1, preferably 8:1 to 4:1; preferably, the molar concentration of Zn is 0.1 to 1.0 mol / L; and the molar concentration of Al is 0.1 to 1.0 mol / L.

[0033] In this invention, the concentration of alkaline substances in alkaline solution d can be selected from a wide range. According to a preferred embodiment of this invention, the molar concentration of alkaline substances in alkaline solution d is 1.0 to 1.5 mol / L.

[0034] In this invention, there are no special requirements for the roasting conditions. Conventional roasting conditions in the art can achieve the purpose of this invention. Preferably, the roasting conditions include: a temperature of 300℃~500℃ and a time of 3-10h.

[0035] In this invention, there is no particular limitation on the type of zinc source, which can be any zinc-containing substance conventional in the art. Preferably, in solutions a and c, the zinc is independently derived from one or more of zinc nitrate hexahydrate, zinc sulfate, and zinc acetate.

[0036] In this invention, the range of alkaline substances that can be selected is relatively wide. Preferably, in alkaline solutions b and d, the alkaline substances are each independently selected from one or more of sodium carbonate, sodium bicarbonate and ammonium carbonate.

[0037] In this invention, there is no particular limitation on the type of aluminum source, which can be any aluminum-containing material conventional in the art. Preferably, in solutions a and c, the aluminum comes from one or both of aluminum nitrate nonahydrate and aluminum sulfate.

[0038] According to a preferred embodiment of the present invention, in step (2), the zinc oxide content in the zinc oxide and aluminum oxide components is 70% to 90% and the aluminum oxide content is 10% to 30% by mass fraction.

[0039] A third aspect of this invention provides the application of the desulfurization adsorbent described herein in the desulfurization of H2S-containing materials. The desulfurization adsorbent described herein, when used for the desulfurization of H2S-containing materials, facilitates the diffusion of H2S, thus exhibiting greater sulfur capacity and higher utilization rate of active components, making it particularly suitable for desulfurization at room temperature.

[0040] In this invention, there is no particular limitation on the type of material, such as natural gas, syngas, coke oven gas or liquid hydrocarbon material.

[0041] The present invention will be described in detail below through embodiments, but the scope of the present invention is not limited to the scope covered by the embodiments.

[0042] In the following examples, the utilization rate of the active component refers to the measured sulfur capacity divided by the theoretical sulfur capacity (the theoretical sulfur capacity calculated based on the zinc content in the adsorbent).

[0043] In the following examples, the specific surface area and pore volume were determined by measuring the N2 adsorption-desorption isotherm of the sample on a Micromeritics TriStar 3000 adsorption instrument, calculating the specific surface area of ​​the sample using the BET formula, and calculating the total pore volume of the sample based on the amount of nitrogen adsorbed at a relative pressure of 0.99.

[0044] XRD patterns were determined using a Rigaku D / MAX-1400 X-ray powder diffractometer (Japan). Cu Kα lines were used as the X-ray source. A nickel filter was used, with a 2θ scanning range of 5–70°, an operating voltage of 40 kV, a current of 40 mA, and a scanning rate of 10° / min to obtain XRD patterns. The grain size was calculated using the Scherrer formula based on the full width at half maximum (FWHM) of the ZnO(100) crystal plane diffraction peaks in the XRD diffraction pattern.

[0045] Example 1

[0046] (1) Add 200 ml of distilled water to a 2000 ml coprecipitation reactor, and add a mixed solution of 0.5 mol / L zinc nitrate hexahydrate and 0.5 mol / L aluminum nitrate nonahydrate at a rate of 30 ml / min, while simultaneously adding 1.7 mol / L sodium carbonate solution dropwise, maintaining pH = 10. After 30 minutes of addition, react at 70 °C for 1 hour, filter, and dry at 120 °C to obtain zinc aluminum hydrotalcite (structural formula Zn). 0.61 Al 0.39 (OH)2(CO3) 0.195 ·4H2O).

[0047] (2) Add 200 ml of distilled water to a 2000 ml coprecipitation reactor, add a mixed solution of 0.8 mol / L zinc nitrate hexahydrate and 0.2 mol / L aluminum nitrate at a rate of 30 ml / min, and add 1.2 mol / L sodium carbonate solution dropwise at the same time, keep the pH = 7, add the material over 30 minutes, after the addition is complete, react at 70 °C for 1 hour, filter, dry at 120 °C, and calcine at 350 °C for 5 hours to obtain component B, in which the mass content of zinc oxide is 72%, the content of aluminum oxide is 18%, and the particle size of zinc oxide is 10 nm.

[0048] (3) 20 parts of zinc-aluminum hydrotalcite and 80 parts of component B were mixed and molded to obtain a desulfurization adsorbent. The desulfurization adsorbent contained 20 parts of zinc-aluminum hydrotalcite, 69 parts of zinc oxide, and 11 parts of aluminum oxide. The specific surface area of ​​the adsorbent was 180 m². 2 / g, pore volume 0.35cm 3 / g.

[0049] In the XRD pattern of the desulfurization adsorbent, I(003) / I(100) = 6.2.

[0050] Catalyst evaluation: The desulfurization adsorbent particles were ground to 20-40 mesh, and 5g was weighed and loaded into a fixed-bed reactor. Under normal temperature and pressure, nitrogen gas containing 5000 μmol / mol H2S was introduced at a rate of 100 ml / min. The H2S concentration at the bed outlet was detected using GC-SCD. When the H2S outlet concentration exceeded 1 μmol / mol, the adsorbent breakthrough occurred. The sulfur capacity of the adsorbent was calculated based on the breakthrough time. The sulfur capacity of the desulfurization adsorbent was 26%; the utilization rate of the active component was 82%.

[0051] Example 2

[0052] (1) Add 200 ml of distilled water to a 2000 ml co-precipitation reactor, and add a mixed solution of 0.3 mol / L zinc nitrate hexahydrate and 0.7 mol / L aluminum nitrate nonahydrate at a rate of 30 ml / min. At the same time, add 1.7 mol / L sodium carbonate solution dropwise, maintain pH = 11, and add the solution over 30 minutes. After the addition is complete, react at 90 °C for 1 hour, filter, and dry at 120 °C to obtain zinc aluminum hydrotalcite (structural formula Zn). 0.56 Al 0.44 (OH)2(CO3) 0.22 ·3H2O).

[0053] (2) Add 200 ml of distilled water to a 2000 ml coprecipitation reactor, add a mixed solution of 0.8 mol / L zinc nitrate hexahydrate and 0.2 mol / L aluminum nitrate at a rate of 30 ml / min, and add 1.2 mol / L sodium carbonate solution dropwise at the same time, keep the pH = 7, add the material over 30 minutes, after the addition is complete, react at 70 °C for 1 hour, filter, dry at 120 °C, and calcine at 350 °C for 5 hours to obtain component B, in which the mass content of zinc oxide is 72%, the content of aluminum oxide is 18%, and the particle size of zinc oxide is 10 nm.

[0054] (3) 20 parts of zinc-aluminum hydrotalcite and 80 parts of component B were mixed and molded to obtain a desulfurization adsorbent. The desulfurization adsorbent contained 20 parts of zinc-aluminum hydrotalcite, 69 parts of zinc oxide, and 11 parts of aluminum oxide. The specific surface area of ​​the adsorbent was 187 m². 2 / g, pore volume 0.36cm 3 / g.

[0055] In the XRD pattern of the desulfurization adsorbent, I(003) / I(100) = 6.4.

[0056] The evaluation method for the desulfurization adsorbent is the same as in Example 1. The sulfur capacity of the desulfurization adsorbent is 27%; the utilization rate of the active component is 85%.

[0057] Example 3

[0058] (1) Add 200 ml of distilled water to a 2000 ml coprecipitation reactor, and add a mixed solution of 0.6 mol / L zinc nitrate hexahydrate and 0.4 mol / L aluminum nitrate nonahydrate at a rate of 30 ml / min. At the same time, add 1.7 mol / L sodium carbonate solution dropwise, maintain pH = 9, and add the solution over 30 minutes. After the addition is complete, react at 50 °C for 1 hour, filter, and dry at 120 °C to obtain zinc aluminum hydrotalcite (structural formula Zn). 0.7 Al 0.3 (OH)2(CO3) 0.15 ·4H2O).

[0059] (2) Add 200 ml of distilled water to a 2000 ml coprecipitation reactor, add a mixed solution of 0.8 mol / L zinc nitrate hexahydrate and 0.2 mol / L aluminum nitrate at a rate of 30 ml / min, and add 1.2 mol / L sodium carbonate solution dropwise at the same time, keep the pH = 7, add the material over 30 minutes, after the addition is complete, react at 70 °C for 1 hour, filter, dry at 120 °C, and calcine at 350 °C for 5 hours to obtain component B, in which the mass content of zinc oxide is 72%, the content of aluminum oxide is 18%, and the particle size of zinc oxide is 10 nm.

[0060] (3) 25 parts of zinc-aluminum hydrotalcite and 75 parts of component B were mixed and molded to obtain a desulfurization adsorbent. The desulfurization adsorbent contained 25 parts of zinc-aluminum hydrotalcite, 65 parts of zinc oxide, and 10 parts of aluminum oxide. The specific surface area of ​​the adsorbent was 195 m². 2 / g, pore volume 0.38cm 3 / g.

[0061] In the XRD pattern of the desulfurization adsorbent, I(003) / I(100) = 6.7.

[0062] The evaluation method for the desulfurization adsorbent is the same as in Example 1. The sulfur capacity of the desulfurization adsorbent is 25%, and the utilization rate of the active component is 81%.

[0063] Example 4

[0064] The method of Example 1 is the same, except that in step (3), 15 parts of zinc-aluminum hydrotalcite are mixed with 85 parts of component B to form a desulfurization adsorbent under the same conditions as in Example 1.

[0065] The desulfurization adsorbent contains 15 parts zinc-aluminum hydrotalcite, 73 parts zinc oxide, and 12 parts aluminum oxide. The specific surface area of ​​the adsorbent is 162 m². 2 / g, pore volume 0.32cm 3 / g.

[0066] In the XRD pattern of the desulfurization adsorbent, I(003) / I(100) = 5.8.

[0067] The evaluation method for the desulfurization adsorbent is the same as in Example 1. The sulfur capacity of the desulfurization adsorbent is 24%, and the utilization rate of the active component is 75%.

[0068] Example 5

[0069] Following the method of Example 1, except that in step (2), 200 ml of distilled water was added to a 2000 ml co-precipitation reactor, and a mixed solution of 0.9 mol / L zinc nitrate hexahydrate and 0.1 mol / L aluminum nitrate was added at a rate of 30 ml / min, while 1.2 mol / L sodium carbonate solution was added dropwise to maintain pH = 7. The addition was carried out over 30 minutes. After the addition was completed, the reaction was carried out at 70°C for 1 hour, filtered, dried at 120°C, and calcined at 350°C for 5 hours to obtain component B, in which the zinc oxide mass content was 72%, the aluminum oxide content was 18%, and the zinc oxide crystal particle size was 12 nm. The remaining conditions were the same as in Example 1 to obtain the desulfurization adsorbent.

[0070] The desulfurization adsorption process contains 20 parts zinc-aluminum hydrotalcite, 73 parts zinc oxide, and 12 parts aluminum oxide. The specific surface area of ​​the adsorbent is 162 m². 2 / g, pore volume 0.32cm 3 / g.

[0071] In the XRD pattern of the desulfurization adsorbent, I(003) / I(100) = 6.2.

[0072] The evaluation method for the desulfurization adsorbent is the same as in Example 1. The sulfur capacity of the desulfurization adsorbent is 25%; the utilization rate of the active component is 74%.

[0073] Comparative Example 1

[0074] The method of Example 1 is followed, except that zinc-aluminum hydrotalcite is not added in step (3), and the other conditions are the same as in Example 1; thus, a desulfurization adsorbent is obtained.

[0075] The desulfurization adsorbent contains 0 parts zinc-aluminum hydrotalcite, 86 parts zinc oxide, and 14 parts aluminum oxide. The specific surface area of ​​the adsorbent is 136 m². 2 / g, pore volume 0.27cm 3 / g.

[0076] In the XRD pattern of the desulfurization adsorbent, I(003) / I(100)=0.

[0077] The evaluation method for the desulfurization adsorbent is the same as in Example 1. The sulfur capacity of the desulfurization adsorbent is 20%, and the utilization rate of the active component is 58%.

[0078] Comparative Example 2

[0079] The method is the same as in Example 1, except that the zinc-aluminum hydrotalcite has the structural formula Zn. 0.8 Al 0.2 (OH)2(CO3) 0.1 ·4H2O, with the remaining conditions the same as in Example 1; to obtain the desulfurization adsorbent.

[0080] The desulfurization adsorbent contains 20 parts zinc-aluminum hydrotalcite, 69 parts zinc oxide, and 11 parts aluminum oxide. The specific surface area of ​​the adsorbent is 147 m². 2 / g, pore volume 0.29cm 3 / g.

[0081] In the XRD pattern of the desulfurization adsorbent, I(003) / I(100) = 6.0.

[0082] The evaluation method for the desulfurization adsorbent is the same as in Example 1. The sulfur capacity of the desulfurization adsorbent is 22%; the utilization rate of the active component is 69%.

[0083] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A desulfurization adsorbent, characterized in that, By weight, the desulfurization adsorbent contains: A) 15-30 parts zinc-aluminum hydrotalcite; B) 50-90 parts zinc oxide; C) 1-15 parts aluminum oxide; The zinc-aluminum hydrotalcite has the structural formula Zn 1-x Al x (OH)2(CO3) x / 2 •nH2O, where x is 0.30~0.44 and n is an integer from 3 to 6; In the XRD pattern of the desulfurization adsorbent, the I(003) / I(100) ratio is 5.6~6.8; the specific surface area of ​​the desulfurization adsorbent is 150-200 m². 2 / g, pore volume greater than 0.3-0.5 cm³ 3 / g; the zinc oxide grain size is 8~11 nm; The preparation method of the zinc-aluminum hydrotalcite includes: The zinc-aluminum hydrotalcite is obtained by first co-precipitation of zinc-aluminum solution a and alkaline solution b, followed by separation and drying. In solution a, the molar ratio of Zn:Al is 7:3 to 3:

7. In alkaline solution b, the alkaline substance is selected from at least one of alkaline carbonates or bicarbonates. The first coprecipitation conditions include: pH 8-12; temperature 40-90℃; time 0.5-3 hours; in solution a, the molar concentration of Zn is 0.1-1.0 mol / L; the molar concentration of Al is 0.1-1.0 mol / L; and in alkaline solution b, the molar concentration of alkaline substances is 1.5-2.0 mol / L. The preparation method of zinc oxide and aluminum oxide includes: subjecting a solution c containing zinc and aluminum and an alkaline solution d to a second co-precipitation to obtain a mixed solution, filtering, drying, and calcining to obtain a component containing zinc oxide and aluminum oxide; the second coprecipitation conditions include: pH 5-9; temperature 40-90℃; time 0.5-3 hours; in solution c, the molar ratio of Zn:Al is 10:1-4:1; in the alkaline solution d, the molar concentration of the alkaline substance is 1.0-1.5 mol / L.

2. The desulfurization adsorbent according to claim 1, wherein, By weight, the content of zinc-aluminum hydrotalcite is 18-25 parts, the content of zinc oxide is 55-85 parts, and the content of aluminum oxide is 2-13 parts.

3. A method for preparing the desulfurization adsorbent according to claim 1 or 2, characterized in that, The method includes: (1) The zinc-aluminum hydrotalcite is obtained by first co-precipitation of zinc-aluminum solution a and alkaline solution b, followed by separation and drying; in solution a, the molar ratio of Zn:Al is 7:3 to 3:7; in the alkaline solution b, the alkaline substance is selected from at least one of alkaline carbonate or bicarbonate. (2) The solution containing zinc and aluminum c and the alkaline solution d were subjected to a second co-precipitation to obtain a mixed solution. The solution was then filtered, dried and calcined to obtain a component containing zinc oxide and aluminum oxide. (3) Zinc-aluminum hydrotalcite and components containing zinc oxide and aluminum oxide are mixed and molded to obtain a desulfurization adsorbent; In step (1), the first coprecipitation conditions include: pH 8-12; temperature 40-90℃; and time 0.5-3 hours. In solution a, the molar concentration of Zn is 0.1~1.0 mol / L; the molar concentration of Al is 0.1~1.0 mol / L. In alkaline solution b, the molar concentration of the alkaline substance is 1.5~2.0 mol / L; Step (2), the second coprecipitation conditions include: pH 5~9; temperature 40~90℃; time 0.5~3 hours; In solution c, the molar ratio of Zn:Al is 10:1 to 4:1; In the alkaline solution d, the molar concentration of the alkaline substance is 1.0~1.5 mol / L.

4. The preparation method according to claim 3, wherein, In step (1), the first coprecipitation conditions include a pH of 9-11.

5. The preparation method according to claim 3, wherein, The roasting conditions include: a temperature of 300℃~500℃ and a time of 3-10h.

6. The preparation method according to claim 3, wherein, Step (2), the second coprecipitation conditions include: pH 6-8; and / or In solution c, the molar ratio of Zn:Al is 8:1-4:

1.

7. The preparation method according to claim 3, wherein, In solution c, the molar concentration of Zn is 0.1~1.0 mol / L; the molar concentration of Al is 0.1~1.0 mol / L.

8. The preparation method according to claim 3, wherein, In solutions a and c, zinc is independently derived from one or more of zinc nitrate hexahydrate, zinc sulfate, and zinc acetate; and / or In alkaline solutions b and d, the alkaline substances are each independently selected from one or more of sodium carbonate, sodium bicarbonate, and ammonium carbonate; and / or In solutions a and c, the aluminum comes from one or both of aluminum nitrate nonahydrate and aluminum sulfate.

9. The preparation method according to claim 3, wherein, In step (2), the zinc oxide and aluminum oxide components contain 70% to 90% zinc oxide and 10% to 30% aluminum oxide by mass fraction.

10. The application of the desulfurization adsorbent according to claim 1 or 2 in the desulfurization of H2S-containing materials.

Citation Information

Patent Citations

  • Preparation method of nano zinc oxide mesopore desulfurizer

    CN101337150A

  • Low-temperature fine desulfurizer and its preparation method

    CN102512942A

  • Preparation method of zinc oxide normal-temperature desulfurizing agent

    CN104307318A

  • Sulfur or arsenic adsorption method

    CN105268276A

  • Normal-temperature COS adsorbent as well as preparation method and application thereof

    CN114433006A