Hydrolytic adsorbents, methods of making and using the same
By preparing zinc-aluminum hydrotalcite and basic zinc carbonate-based hydrolytic adsorbent, the problem of COS and CS₂ being difficult to remove in one step was solved, achieving a highly efficient one-step desulfurization effect, simplifying the process and improving desulfurization efficiency.
Patent Information
- Application Number
- CN202211289331.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-20
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-10-20
AI Technical Summary
In existing technologies, COS and CS₂ are difficult to remove in one step and need to be hydrolyzed into H₂S before entering subsequent processes for removal, which makes the process complex.
A hydrolytic adsorbent, composed of zinc-aluminum hydrotalcite, basic zinc carbonate, and alkali metals, is prepared by mixing and molding and contacting with alkali metal compounds to form an adsorbent with highly basic centers. This adsorbent can directly hydrolyze COS and CS₂ to generate H₂S and adsorb them, achieving one-step removal.
It achieves efficient one-step removal of COS and CS₂, simplifies the process, and improves desulfurization efficiency and sulfur capacity.
Smart Images

Figure CN117917461B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of oil and gas purification technology, specifically to a hydrolysis adsorbent, its preparation method, and its application. Background Technology
[0002] Natural gas, syngas, coke oven gas, and liquid hydrocarbon feedstocks typically contain impurities such as COS and CS2. The presence of these impurities can poison the catalysts in subsequent reaction units, affecting the long-term stable operation of the plant. Methods for removing COS and CS2 include adsorption, hydroconversion, and hydrolysis. Hydrolysis is widely used industrially due to its advantages of mild reaction conditions, fewer side reactions, and relatively low energy consumption. Hydrolysis involves reacting COS and CS2 with H2O on a catalyst to generate H2S. The H2S is then further removed in subsequent stages using dry or wet methods. This requires at least two units connected in series in the system to effectively remove sulfur-containing impurities, making the process complex. Therefore, developing integrated hydrolysis and adsorption agents is of great significance.
[0003] CN101031350A discloses a method for removing COS from a syngas stream containing H2S and COS. The method includes the following steps: (a) converting COS in the first syngas stream to H2S by contacting it with a COS hydrolysis catalyst in the presence of water in a hydrolysis zone, thereby obtaining a second syngas stream that is COS-poor and H2S-rich; (b) removing H2S from the second syngas stream by contacting it with a solid adsorbent during H2S removal, thereby obtaining a third syngas stream that is H2S-poor and COS-poor. This method involves hydrolyzing COS before adsorption and removal in the next zone.
[0004] CN100431668C discloses a COS and CS2 hydrolysis catalyst and its application. This invention uses ammonium salts supported on alumina to prepare the hydrolysis catalyst, solving the problem that existing desulfurizing agents cannot remove organic sulfur with high precision. This invention hydrolyzes COS and CS2 into H2S, which is then removed in subsequent processes.
[0005] CN102600850B discloses a method for preparing an activated carbon-based catalyst that simultaneously removes carbonyl sulfide and carbon disulfide. This method uses microwave-activated carbon as a support and alkaline substances and metal oxides as active components to prepare an activated carbon-based catalyst capable of simultaneously removing carbonyl sulfide and carbon disulfide. This catalyst can simultaneously remove COS and CS2 from gases at relatively low temperatures (30–90°C), along with their byproducts. The method is simple, easy to operate, and has low operating costs. It achieves high COS and CS2 removal efficiency, with conversion rates exceeding 90% for both COS and CS2. The method involves hydrolyzing COS and CS2 into H2S for subsequent removal in a later process. Summary of the Invention
[0006] The purpose of this invention is to overcome the problem that COS and CS2 are difficult to remove in one step in the existing technology and need to be hydrolyzed into H2S before entering the subsequent process for removal. The invention provides a hydrolytic adsorbent that is used for desulfurization and has the advantage of high sulfur capacity. It is used to remove COS and CS2 and can directly remove sulfur-containing impurities in the raw materials in one step.
[0007] To achieve the above objectives, the first aspect of the present invention provides a hydrolytic adsorbent, which, by weight, contains: a) 30 to 70 parts of zinc aluminum hydrotalcite; b) 30 to 70 parts of basic zinc carbonate; and c) 0.1 to 8 parts of alkali metal.
[0008] A second aspect of the present invention provides a method for preparing the hydrolysis adsorbent of the present invention, the method comprising:
[0009] (1) Zinc aluminum hydrotalcite and basic zinc carbonate are mixed and molded to obtain an adsorbent precursor;
[0010] (2) The adsorbent precursor is contacted with a solution containing an alkali metal compound and dried to obtain a hydrolytic adsorbent.
[0011] A third aspect of the present invention provides the application of the hydrolytic adsorbent described herein in the desulfurization of feedstocks containing COS and / or CS2.
[0012] Through the above technical solution, the hydrolytic adsorbent provided by the present invention is used for desulfurization of raw materials containing COS and / or CS2. The layered structure of zinc-aluminum hydrotalcite is conducive to the diffusion of COS and CS2. Zinc-aluminum hydrotalcite, together with basic zinc carbonate and alkali metals, increases the alkaline centers of the adsorbent and improves the hydrolysis performance. At the same time, zinc-aluminum hydrotalcite and basic zinc carbonate can directly adsorb H2S generated by the hydrolysis of COS and CS2, achieving the effect of directly removing sulfur-containing impurities from the raw materials in one step. Attached Figure Description
[0013] Figure 1 This is the XRD pattern of the hydrolysis adsorbent prepared in Example 1;
[0014] Figure 2 This is a scanning electron microscope (SEM) image of the hydrolysis adsorbent prepared in Example 1. Detailed Implementation
[0015] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0016] In this invention, I(003) / I(200) refers to the ratio of the intensity of the (003) crystal plane diffraction peak to the intensity of the (200) crystal plane diffraction peak in the XRD pattern of the hydrolytic adsorbent.
[0017] The first aspect of this invention provides a hydrolytic adsorbent, comprising, by weight: a) 30-70 parts of zinc aluminum hydrotalcite; b) 30-70 parts of basic zinc carbonate; and c) 0.1-8 parts of alkali metal hydroxide; wherein the alkali metal hydroxide is calculated as an alkali metal. In this invention, the zinc aluminum hydrotalcite, basic zinc carbonate, and alkali metal work together to increase the alkalinity of the adsorbent.
[0018] According to a preferred embodiment of the present invention, in the XRD pattern of the hydrolytic adsorbent, I(003) / I(200) is 15 to 1.
[0019] According to a preferred embodiment of the present invention, the weak base concentration of the hydrolytic adsorbent is not less than 0.70 mmol / g, and preferably not more than 1 mmol / g.
[0020] In this invention, layered zinc-aluminum hydrotalcites can all be used. According to a preferred embodiment of this invention, the zinc-aluminum hydrotalcite has the structural formula Zn. 1-x Al x (OH)2(CO3) x / 2 ·nH2O, where x is 0.30 to 0.44 and n is an integer from 3 to 6; this is conducive to the diffusion of COS and CS2.
[0021] In this invention, a wide range of alkali metals can be selected. According to a preferred embodiment of this invention, the alkali metal is selected from at least one of Li, Na, K, Rb and Cs.
[0022] According to a preferred embodiment of the present invention, the hydrolytic adsorbent contains, by weight, a) 35-65 parts of zinc aluminum hydrotalcite; b) 35-65 parts of basic zinc carbonate; and 1-6 parts of alkali metal.
[0023] Hydrolyzing adsorbents possessing the aforementioned properties can achieve the objectives of this invention. This invention does not impose particular requirements on the preparation method of the hydrolyzing adsorbent. According to a preferred embodiment of this invention, this invention provides a method for preparing the hydrolyzing adsorbent described above, the method comprising:
[0024] (1) Zinc aluminum hydrotalcite and basic zinc carbonate are mixed and molded to obtain an adsorbent precursor;
[0025] (2) The adsorbent precursor is contacted with an alkali metal hydroxide and dried to obtain a hydrolyzed adsorbent.
[0026] In this invention, layered zinc-aluminum hydrotalcites can all be used. According to a preferred embodiment of this invention, the zinc-aluminum hydrotalcite has the structural formula Zn. 1-x Al x (OH)2(CO3) x / 2 ·nH2O, where x is 0.30 to 0.44 and n is an integer from 3 to 6; the preparation method of the zinc-aluminum hydrotalcite includes: separating and drying the zinc-aluminum hydrotalcite after co-precipitating a solution I containing zinc and aluminum and an alkaline solution II, wherein the alkaline substance in the alkaline solution II is selected from at least one of carbonates or bicarbonates.
[0027] According to a preferred embodiment of the present invention, the first coprecipitation conditions include: pH 8-12, preferably 9-11; temperature 40-90°C; and time 0.5-3 hours.
[0028] In this invention, the concentrations of zinc and aluminum in solution I can be selected within a wide range. According to a preferred embodiment of this invention, in solution I containing zinc and aluminum, the molar ratio of Zn:Al is 7:3 to 3:7; the molar concentration of Zn is 0.1 to 1.0 mol / L; and the molar concentration of Al is 0.1 to 1.0 mol / L.
[0029] In this invention, the concentration of alkaline substance in alkaline solution II can be selected from a wide range. According to a preferred embodiment of this invention, the molar concentration of alkaline substance in alkaline solution II is 1.5 to 2.0 mol / L.
[0030] In this invention, there are no special requirements for the preparation method of the basic zinc carbonate. According to a preferred embodiment of the present invention, the present invention provides a method for preparing the basic zinc carbonate, the method comprising: separating and drying a zinc-containing solution III and an alkaline solution IV in a co-current flow for a second co-precipitation to obtain the basic zinc carbonate.
[0031] According to a preferred embodiment of the present invention, the second coprecipitation conditions include: pH 5-9, preferably 6-8; temperature 40-90°C; and time 0.5-3 hours.
[0032] In this invention, the zinc concentration in the zinc-containing solution III can be selected from a wide range. According to a preferred embodiment of this invention, the molar concentration of Zn in the zinc-containing solution III is 0.1 to 1 mol / L.
[0033] In this invention, the concentration of alkaline substances in alkaline solution IV can be selected from a wide range. According to a preferred embodiment of this invention, the molar concentration of alkaline substances in alkaline solution IV is 1.0 to 1.5 mol / L.
[0034] In this invention, in step (2), the adsorbent precursor is contacted with a solution containing an alkali metal compound. The contact method can be impregnation, preferably equal-volume impregnation. The concentration of the alkali metal in the solution can be selected over a wide range, for example, it can be calculated based on the weight parts of the alkali metal and the impregnation volume of the solution.
[0035] In this invention, there is no particular limitation on the type of zinc source, which can be any zinc-containing substance conventional in the art. Preferably, in the zinc and aluminum-containing solution I and the zinc-containing solution III, the zinc is independently derived from one or more of zinc nitrate hexahydrate, zinc sulfate, and zinc acetate.
[0036] In this invention, the range of alkaline substances that can be selected is relatively wide. Preferably, in alkaline solution II and alkaline solution IV, the alkaline substances are each independently selected from one or more of sodium carbonate, sodium bicarbonate and ammonium carbonate.
[0037] In this invention, there is no particular limitation on the type of aluminum source, which can be any aluminum-containing material conventional in the art. Preferably, in the zinc and aluminum-containing solution I, the aluminum comes from one or both of aluminum nitrate nonahydrate and aluminum sulfate.
[0038] A third aspect of this invention provides the application of the hydrolytic adsorbent described herein in the desulfurization of feedstocks containing COS and / or CS2. The hydrolytic adsorbent provided by this invention is used for the desulfurization of feedstocks containing COS and / or CS2. The layered structure of zinc-aluminum hydrotalcite facilitates the diffusion of COS and CS2. The combined action of zinc-aluminum hydrotalcite with basic zinc carbonate and alkali metals increases the alkaline centers of the adsorbent, improving hydrolysis performance. Simultaneously, zinc-aluminum hydrotalcite and basic zinc carbonate can directly adsorb H2S generated from the hydrolysis of COS and CS2, achieving the effect of directly removing sulfur-containing impurities from the feedstock in a one-step process.
[0039] In this invention, there is no particular limitation on the type of raw material, such as natural gas, syngas, coke oven gas or liquid hydrocarbon raw material.
[0040] In this invention, the weak base center refers to the base center calculated from the amount of CO2 desorbed at less than 300°C during the programmed temperature desorption process.
[0041] The present invention will be described in detail below through embodiments, but the scope of the present invention is not limited to the scope covered by the embodiments.
[0042] In the following examples, the alkalinity of the sample's alkaline center was determined using a self-made temperature-programmed thermal desorption device. The CO2 adsorption temperature was 100°C, the carrier gas was He, and the flow rate was 30 mL / min. -1 After adsorption saturation, helium gas was used for purging, and the programmed heating rate was 10℃·min. -1 The temperature is raised to 300℃, and the amount of carbon dioxide adsorbed is weighed using a microbalance. The amount of weak base center of the adsorbent is also calculated.
[0043] XRD patterns were determined using a Rigaku D / MAX-1400 X-ray powder diffractometer (Japan). Cu Kα lines were used as the X-ray source. A nickel filter was used to obtain XRD patterns by using a 2θ scanning range of 5–70°, an operating voltage of 40 kV, a current of 40 mA, and a scanning rate of 10° / min.
[0044] Example 1
[0045] (1) Add 200 ml of distilled water to a 2000 ml coprecipitation reactor, and add a mixed solution of 0.5 mol / L zinc nitrate hexahydrate and 0.5 mol / L aluminum nitrate nonahydrate at a rate of 30 ml / min. At the same time, add 1.7 mol / L sodium carbonate solution dropwise, maintain pH = 10, and add the solution over 30 minutes. After the addition is complete, react at 70 °C for 1 hour, filter, and dry at 120 °C to obtain zinc aluminum hydrotalcite A (structural formula Zn). 0.61 Al 0.39 (OH)2(CO3) 0.195 ·4H2O).
[0046] (2) Add 200ml of distilled water to a 2000ml coprecipitation reactor, add 0.8mol / L zinc nitrate hexahydrate at a rate of 30ml / min, and add 1.2mol / L sodium carbonate solution dropwise at the same time, keep the pH=7, add the material for 30 minutes, after the addition is complete, react at 70℃ for 1 hour, filter, and dry at 120℃ to obtain basic zinc carbonate component B.
[0047] (3) Mix 50 parts of zinc-aluminum hydrotalcite A with 50 parts of basic zinc carbonate component B to form an adsorbent precursor. Dissolve 4 parts of potassium hydroxide in 100 parts of water and immerse adsorbent particles C in it. Dry at 120°C to obtain hydrolyzed adsorbent particles.
[0048] According to XRD data, the I(003) / I(200) ratio in the hydrolytic adsorbent is 9.7.
[0049] The weak base center of the hydrolytic adsorbent has an alkalinity of 0.92 mmol / g.
[0050] Evaluation of the hydrolysis adsorbent: The hydrolysis adsorbent particles were ground to 20-40 mesh, and 3g was weighed and loaded into a fixed-bed reactor. Under normal pressure and at 180℃, nitrogen gas containing 1000 μmol / mol COS + 200 μmol / mol CS2 was introduced at a rate of 80 ml / min. The water content of the system was mixed with the feed gas by bubbling nitrogen into the reactor. The sulfur content of the tail gas was detected by gas chromatography with an SCD detector. When the outlet concentration of COS, CS2, or H2S exceeded 1 μmol / mol, the adsorbent breakthrough was achieved. The sulfur capacity of the adsorbent was calculated based on the breakthrough time. The sulfur capacity of the adsorbent was 980 mg / g.
[0051] Example 2
[0052] (1) Add 200 ml of distilled water to a 2000 ml coprecipitation reactor, and add a mixed solution of 0.3 mol / L zinc nitrate hexahydrate and 0.7 mol / L aluminum nitrate nonahydrate at a rate of 30 ml / min. At the same time, add 1.7 mol / L sodium carbonate solution dropwise, maintain pH = 11, and add the solution over 30 minutes. After the addition is complete, react at 90 °C for 1 hour, filter, and dry at 120 °C to obtain zinc aluminum hydrotalcite A (structural formula Zn). 0.56 Al 0.44 (OH)2(CO3) 0.22 ·3H2O).
[0053] (2) Add 200ml of distilled water to a 2000ml coprecipitation reactor, add 0.8mol / L zinc nitrate hexahydrate at a rate of 30ml / min, and add 1.2mol / L sodium carbonate solution dropwise at the same time, keep the pH=7, add the material for 30 minutes, after the addition is complete, react at 70℃ for 1 hour, filter, and dry at 120℃ to obtain basic zinc carbonate component B.
[0054] (3) Mix 40 parts of zinc-aluminum hydrotalcite A with 60 parts of basic zinc carbonate component B to form an adsorbent precursor. Dissolve 4 parts of potassium hydroxide in 100 parts of water and impregnate the adsorbent particles C in it. Dry at 120°C to obtain hydrolyzed adsorbent particles.
[0055] According to XRD data, the ratio of I(003) to I(200) in the hydrolytic adsorbent is 7.
[0056] The weak base center of the hydrolytic adsorbent has an alkalinity of 0.94 mmol / g.
[0057] The evaluation method for the hydrolysis adsorbent is the same as in Example 1. The sulfur capacity of the hydrolysis adsorbent is 910 mg / g.
[0058] Example 3
[0059] (1) Add 200 ml of distilled water to a 2000 ml coprecipitation reactor, and add a mixed solution of 0.6 mol / L zinc nitrate hexahydrate and 0.4 mol / L aluminum nitrate nonahydrate at a rate of 30 ml / min. At the same time, add 1.7 mol / L sodium carbonate solution dropwise, maintain pH = 9, and add the solution over 30 minutes. After the addition is complete, react at 50 °C for 1 hour, filter, and dry at 120 °C to obtain zinc aluminum hydrotalcite (structural formula Zn). 0.7 Al 0.3 (OH)2(CO3) 0.15 ·4H2O).
[0060] (2) Add 200ml of distilled water to a 2000ml coprecipitation reactor, add 0.8mol / L zinc nitrate hexahydrate at a rate of 30ml / min, and add 1.2mol / L sodium carbonate solution dropwise at the same time, keep the pH=7, add the material for 30 minutes, after the addition is complete, react at 70℃ for 1 hour, filter, and dry at 120℃ to obtain basic zinc carbonate component B.
[0061] (3) Mix 30 parts of zinc-aluminum hydrotalcite A with 70 parts of basic zinc carbonate component B to form an adsorbent precursor. Dissolve 4 parts of potassium hydroxide in 100 parts of water and impregnate the adsorbent particles C in it. Dry at 120°C to obtain hydrolyzed adsorbent particles.
[0062] According to XRD data, the ratio of I(003) to I(200) in the hydrolytic adsorbent is 2.5.
[0063] The weak base center of the hydrolytic adsorbent has an alkalinity of 0.98 mmol / g.
[0064] The evaluation method for the hydrolysis adsorbent is the same as in Example 1. The sulfur capacity of the hydrolysis adsorbent is 874 mg / g.
[0065] Example 4
[0066] The method of Example 1 differs in that the hydrolytic adsorbent contains 70 parts of zinc aluminum hydrotalcite, 30 parts of basic zinc carbonate component, and 4 parts of potassium.
[0067] According to XRD data, the ratio of I(003) to I(200) in the hydrolytic adsorbent is 15.
[0068] The weak base center of the hydrolytic adsorbent has an alkalinity of 0.89 mmol / g.
[0069] The evaluation method for the hydrolysis adsorbent is the same as in Example 1. The sulfur capacity of the hydrolysis adsorbent is 943 mg / g.
[0070] Example 5
[0071] The method is the same as in Example 1, except that in step (3), the amount of potassium alkali metal added is 1 part, and the other conditions are the same as in Example 1.
[0072] According to XRD data, the I(003) / I(200) ratio in the hydrolytic adsorbent is 9.7.
[0073] The weak base center of the hydrolytic adsorbent has an alkalinity of 0.75 mmol / g.
[0074] The evaluation method for the hydrolysis adsorbent is the same as in Example 1. The sulfur capacity of the hydrolysis adsorbent is 810 mg / g.
[0075] Example 6
[0076] The method is the same as in Example 1, except that in step (3), the amount of potassium alkali metal added is 8 parts, and the other conditions are the same as in Example 1.
[0077] According to XRD data, the I(003) / I(200) ratio in the hydrolytic adsorbent is 9.7.
[0078] The weak base center of the hydrolytic adsorbent has an alkalinity of 0.98 mmol / g.
[0079] The evaluation method for the hydrolysis adsorbent is the same as in Example 1. The sulfur capacity of the hydrolysis adsorbent is 965 mg / g.
[0080] Comparative Example 1
[0081] The method is the same as in Example 1, except that zinc-aluminum hydrotalcite is not added in step (3), and the other conditions are the same as in Example 1.
[0082] According to XRD data, the ratio of I(003) / I(200) in the hydrolysis adsorbent is 0.
[0083] The weak base center of the hydrolytic adsorbent has an alkalinity of 0.89 mmol / g.
[0084] The evaluation method for the hydrolysis adsorbent is the same as in Example 1. The sulfur capacity of the hydrolysis adsorbent is 748 mg / g.
[0085] Comparative Example 2
[0086] The method is the same as in Example 1, except that no alkali metal is added in step (3), while the other conditions are the same as in Example 1.
[0087] The XRD data for the hydrolyzed adsorbent, I(003) / I(200), is 9.7.
[0088] The weak base center of the hydrolytic adsorbent has an alkalinity of 0.58 mmol / g.
[0089] The evaluation method for the hydrolysis adsorbent is the same as in Example 1. The sulfur capacity of the hydrolysis adsorbent is 698 mg / g.
[0090] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A hydrolytic adsorbent, characterized in that, The hydrolytic adsorbent comprises, by weight parts: a) 30-70 parts of zinc-aluminum hydrotalcite; b) 30-70 parts of basic zinc carbonate; c) 0.1-8 parts of alkali metal; the structural formula of the zinc-aluminum hydrotalcite is Zn 1-x Al x (OH)2(CO3) x / 2 •nH2O, wherein x is 0.30-0.44, n is an integer of 3-6; the I(003) / I(200) of the hydrolytic adsorbent XRD pattern is 15-1; The weak base concentration of the hydrolytic adsorbent is not less than 0.70 mmol / g and not more than 1 mmol / g. The preparation method of the zinc-aluminum hydrotalcite includes: co-currently running a zinc-aluminum solution I and an alkaline solution II for a first coprecipitation, separating and drying the solutions to obtain the zinc-aluminum hydrotalcite; in the alkaline solution II, the alkaline substance is selected from at least one of carbonates or bicarbonates; the first coprecipitation conditions include: pH 8-12; temperature 40-90℃; time 0.5-3 hours; In solution I containing zinc and aluminum, the molar ratio of Zn:Al is 7:3 to 3:7; the molar concentration of Zn is 0.1 to 1.0 mol / L; and the molar concentration of Al is 0.1 to 1.0 mol / L. In alkaline solution II, the molar concentration of the alkaline substance is 1.5~2.0 mol / L.
2. The hydrolysis adsorbent according to claim 1, wherein, The alkali metal is selected from at least one of Li, Na, K, Rb and Cs.
3. The hydrolysis adsorbent according to claim 1 or 2, wherein, By weight, the hydrolytic adsorbent contains a) 35-65 parts zinc aluminum hydrotalcite; b) 35-65 parts basic zinc carbonate; and c) 1-6 parts alkali metals.
4. A method for preparing the hydrolysis adsorbent according to any one of claims 1-3, characterized in that, The method includes: (1) Zinc-aluminum hydrotalcite and basic zinc carbonate are mixed and molded to obtain an adsorbent precursor; (2) The adsorbent precursor is contacted with a solution containing an alkali metal compound and dried to obtain a hydrolytic adsorbent; The preparation method of the zinc-aluminum hydrotalcite includes: co-currently running a zinc-aluminum solution I and an alkaline solution II for a first coprecipitation, separating and drying the solutions to obtain the zinc-aluminum hydrotalcite; in the alkaline solution II, the alkaline substance is selected from at least one of carbonates or bicarbonates; the first coprecipitation conditions include: pH 8-12; temperature 40-90℃; time 0.5-3 hours; In solution I containing zinc and aluminum, the molar ratio of Zn:Al is 7:3 to 3:7; the molar concentration of Zn is 0.1 to 1.0 mol / L; and the molar concentration of Al is 0.1 to 1.0 mol / L. In alkaline solution II, the molar concentration of the alkaline substance is 1.5~2.0 mol / L.
5. The preparation method according to claim 4, wherein, The first coprecipitation conditions include a pH of 9-11.
6. The preparation method according to claim 4, wherein, The preparation method of the basic zinc carbonate includes: co-precipitating zinc-containing solution III and alkaline solution IV in a second co-precipitation, separating and drying to obtain the basic zinc carbonate.
7. The preparation method according to claim 6, wherein, The second coprecipitation conditions include: pH 5–9; temperature 40–90°C; time 0.5–3 hours; and / or In zinc-containing solution III, the molar concentration of Zn is 0.1–1.0 mol / L; and / or In alkaline solution IV, the molar concentration of the alkaline substance is 1.0~1.5 mol / L.
8. The preparation method according to claim 6, wherein, The second coprecipitation conditions include a pH of 6 to 8.
9. The application of the hydrolytic adsorbent according to any one of claims 1-3 in the desulfurization of feedstocks containing COS and / or CS2.
Citation Information
Patent Citations
Hydrolyst for COS and CS2 and application thereof
CN100431668C
Process for the removal of cos from a synthesis gas stream comprising h2s and cos
CN101031350A
Preparation method of a catalyst for simultaneously removing carbonyl sulfide and carbon disulfide
CN102600850B
Sulfur or arsenic adsorption method
CN105268276A
Normal-temperature COS adsorbent as well as preparation method and application thereof
CN114433006A