Preparation method of composite dehumidification runner and composite dehumidification runner

By using molecular sieves and polymer composites to prepare dehumidifying rotors, the problems of adsorbent shedding and high energy consumption caused by glass fiber substrates are solved, achieving efficient and stable dehumidification performance and long-life rotors.

CN117919904BActive Publication Date: 2026-11-24QINGDAO HUASHIJIE ENVIRONMENT TECHNOLOGY CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211262110.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-14
Publication Date
2026-11-24
Estimated Expiration
2042-10-14

AI Technical Summary

Technical Problem

Existing dehumidification rotors have a high proportion of fiberglass substrate, and the adsorbent is prone to falling off, resulting in low dehumidification efficiency, high energy consumption and short lifespan. Traditional coating methods have weak material interaction, which affects the performance of the rotor.

Method used

A composite dehumidification rotor is prepared by using molecular sieves as the adsorbent and polymers as the carrier, through activation, pretreatment and polymerization molding. This avoids the use of glass fiber substrates, improves the binding strength and adsorption capacity of the adsorbent, and reduces desorption energy consumption.

Benefits of technology

It improves the efficiency and lifespan of the dehumidification rotor, reduces operating energy consumption, avoids the risk of adsorbent shedding, and achieves stable dehumidification performance under different humidity conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117919904B_ABST
    Figure CN117919904B_ABST
Patent Text Reader

Abstract

This invention provides a method for preparing a composite dehumidifying rotor and the composite dehumidifying rotor itself, belonging to the field of dehumidifying rotor manufacturing. The preparation method involves activating and pretreating molecular sieve powder; adding activated carbon to an acrylic acid solution to remove polymerization inhibitors; adding an alkaline solution to the supernatant obtained after separation for neutralization to obtain a neutralized solution; adding the pretreated molecular sieve and crosslinking agent to the neutralized solution; heating and adding an initiator while stirring until homogeneous; controlling the polymerization temperature until a gel-like state is achieved; extruding the gel-like product into honeycomb blocks; drying the honeycomb blocks, washing, and then performing a second vacuum drying to obtain the composite dehumidifying rotor. The composite dehumidifying rotor prepared using this invention can improve the rotor's water vapor adsorption and desorption efficiency, avoid the risk of adsorbent detachment in traditional coating preparation methods, and the molecular sieve provides a doping enhancement effect that prevents polymer breakage and cracking during the adsorption-desorption process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of dehumidifying impeller manufacturing, specifically, it relates to a method for preparing a composite dehumidifying impeller and the composite dehumidifying impeller itself. Background Technology

[0002] Rotary dehumidification systems are widely used due to their advantages such as energy saving, large dehumidification capacity, high efficiency, and continuous supply of low dew point dry air. In this system, the dehumidification rotor is the heart, making the adsorbent material loaded on it extremely crucial. Currently, adsorbent materials can be divided into two main categories: inorganic and organic. Inorganic adsorbent materials include hygroscopic salts, silica gel, and molecular sieves. Hygroscopic salts such as LiCl, CaCl2, and MgCl2, while possessing large moisture absorption capacity and fast absorption speed, are prone to liquefaction and are difficult to regenerate after moisture absorption. Silica gel, also known as silica gel, is a highly hydrophilic compound whose main chemical component is hydrated silicon dioxide. Although widely used, it still has many shortcomings. For example, compared to lithium chloride, silica gel has a smaller dehumidification capacity and lower dehumidification efficiency, making it unsuitable for high-humidity environments. Furthermore, silica gel requires high regeneration temperatures during regeneration, resulting in high energy consumption. Additionally, the bonding strength between silica gel and the rotor substrate is not high, making it prone to desiccant coating peeling off. In severe cases, pore blockage or collapse can occur, obstructing airflow and affecting dehumidification efficiency. Molecular sieves offer numerous advantages as rotary adsorption materials. They exhibit excellent adsorption performance in environments with low relative humidity (<20% RH), while conventional silica gel adsorbs less than one-third of the molecular sieve's capacity under the same conditions. Furthermore, molecular sieves maintain considerable adsorption capacity at higher temperatures, whereas silica gel adsorption is almost zero at temperatures above 100°C. However, molecular sieves also have drawbacks. Because adsorption is achieved through their regular pore structure, their moisture absorption capacity is lower than conventional adsorption materials like lithium chloride and silica gel. Additionally, desorption from molecular sieves is relatively difficult, requiring high regeneration temperatures and making it challenging to utilize low-temperature heat sources for desorption. Organic hygroscopic materials, on the other hand, are novel functional polymers developed from highly absorbent resins. They possess excellent hygroscopic and moisture-retaining properties. These are water-based resins modified through chemical and physical methods, absorbing moisture through hydrophilic groups in their molecules. Their hygroscopic performance surpasses that of general inorganic materials, with a moisture absorption capacity exceeding 70%. They also feature rapid moisture absorption, low desorption temperatures, and are non-corrosive and non-polluting. However, due to their structure, these materials undergo volume changes during adsorption and desorption. Under high humidity conditions, long-term adsorption and desorption can easily cause damage, and their physical strength is lower than that of inorganic adsorption materials.

[0003] Commonly used dehumidifying impellers mainly consist of a honeycomb impeller substrate, adsorbent material, and a shell. The honeycomb impeller substrate is generally made of fiberglass paper through methods such as rolling, laying, and stacking. The adsorbent material is loaded onto the substrate through physical or chemical means. Currently, the fiberglass substrate accounts for a relatively high proportion within the impeller; for example, the substrate accounts for about 30-40% in silica gel impellers and nearly 50% in molecular sieve impellers. However, the substrate portion does not have adsorption capacity. During the desorption process, the overall temperature of the impeller rises, and the substrate portion increases the energy consumption of the impeller for desorption. For example, the specific heat of the fiberglass substrate is 0.9 kJ·kg. -1 ·K -1 Under normal operating conditions, the sensible heat energy consumption of the substrate accounts for 25-30% of the desorption energy consumption of the dehumidification wheel. In addition, regardless of how the dehumidification material prepared by traditional coating methods is loaded onto the substrate, the material force is relatively weak, and the problem of detachment is unavoidable, which in turn affects the life of the wheel. Summary of the Invention

[0004] The purpose of this invention is to provide a method for preparing a composite dehumidifying rotor and the composite dehumidifying rotor itself, overcoming the defects of current dehumidifying rotor products caused by fiberglass substrates, such as low adsorbent content and the risk of adsorbent shedding. Specifically, the invention uses molecular sieves as the main adsorbent and polymers (resins) as the carrier, directly molding a fully adsorbent composite dehumidifying rotor from polymers and molecular sieves. This invention's fully adsorbent composite dehumidifying rotor does not contain a fiberglass carrier; the rotor, except for the outer shell and bearings, is absorbent, which can improve rotor efficiency, reduce the energy consumption per unit dehumidification capacity, and simultaneously avoid the risk of adsorbent shedding, thus extending rotor life.

[0005] To achieve the above objectives, this invention provides a method for preparing a composite dehumidifying rotor and the composite dehumidifying rotor itself, wherein the preparation method is as follows:

[0006] S1: Activate and pretreat the molecular sieve powder.

[0007] Further, in step S1, the activation of the molecular sieve powder refers to drying the molecular sieve at 250-550℃ and cooling it. Subsequently, it is soaked in a 1-3% alkaline solution for 9-15 hours, washed, and dried. The alkaline solution is preferably a NaOH solution.

[0008] The purpose of activating molecular sieve raw powder is to remove adsorbed water and impurities from the molecular sieve. The purpose of alkaline solution soaking pretreatment includes: 1. Etching the surface of the molecular sieve to improve the bonding force between the molecular sieve and the polymer; 2. After alkaline treatment, some silicon elements in the molecular sieve are converted into SiO3. 2- The form of dissolution can play a role in bonding between inorganic molecular sieve crystals after dehydration in the drying process; third, after alkali treatment, silicon atoms are removed from the molecular sieve framework, thereby introducing mesopores and macropores into the molecular sieve channel system, reducing the silicon-to-aluminum ratio, which can improve the adsorption capacity of the molecular sieve for water and reduce desorption energy consumption.

[0009] Preferably, the activation of the molecular sieve powder in step S1 refers to drying the molecular sieve at 300°C, cooling it, soaking it in a 2% alkaline solution for 12 hours, washing it, and drying it.

[0010] S2: Add activated carbon to the acrylic acid solution to remove the polymerization inhibitor, and add an alkaline solution to the supernatant obtained after separation to carry out a neutralization reaction to obtain a neutralized solution.

[0011] Industrial acrylic acid and its derivatives are generally treated with p-hydroxyanisole MEHQ as a polymerization inhibitor. In this invention, activated carbon is preferred to be used to adsorb and remove the polymerization inhibitor.

[0012] Further, in step S2, the concentration of the acrylic acid solution is 30-50%, preferably 40%.

[0013] Preferably, the concentration of the alkaline solution is 10-30%, more preferably, the concentration of the alkaline solution is 25%. The alkaline solution is preferably a NaOH solution.

[0014] Preferably, the mass ratio of the acrylic acid solution to the alkaline solution is (1-3):1; more preferably, the mass ratio of the acrylic acid solution to the alkaline solution is 1:1.

[0015] Preferably, the neutralization reaction temperature is 15-35°C, and more preferably, the neutralization reaction temperature is 30°C.

[0016] S3: Add the pretreated molecular sieve and crosslinking agent from S1 to the neutralization solution described in S2, heat up, add the initiator and stir until homogeneous, control the polymerization temperature until a gel-like state is achieved, and obtain a polymer containing molecular sieve.

[0017] Further, in step S3, the ratio of the molecular sieve to the acrylic acid solution in step S2 is (5-8):1, more preferably 6:1.

[0018] Preferably, the molecular sieve is a type A molecular sieve or a type X molecular sieve powder.

[0019] Preferably, the crosslinking agent comprises one or more of 1,4-butanediol diacrylate, ethylene glycol dimethacrylate, TAC, butyl acrylate, HEA, HPA, HEMA, HPMA, and MMA.

[0020] Further, the amount of the crosslinking agent is 0.01-0.03% of the acrylic acid solution in step S2, more preferably 0.02%.

[0021] Preferably, the initiator is an inorganic peroxide. More preferably, the inorganic peroxide is ammonium persulfate or potassium persulfate.

[0022] Furthermore, the amount of the initiator is 0.1-0.35% of the acrylic acid solution in step S2, more preferably 0.2%.

[0023] Furthermore, the temperature increase is to 30-40°C, more preferably 35°C.

[0024] The polymerization temperature is 50-75℃, more preferably 65℃; the polymerization reaction time is 2-3h.

[0025] S4: The polymer containing molecular sieves described in S3 is extruded into a honeycomb block.

[0026] S5: After drying the honeycomb block described in S4, wash it and dry it again under vacuum to obtain the final product.

[0027] Furthermore, in step S5, the drying temperature of the honeycomb block is 60-80℃, more preferably 80℃.

[0028] Furthermore, the washing is performed using anhydrous ethanol.

[0029] Furthermore, the temperature for the secondary drying under vacuum is 60-80°C, more preferably 80°C.

[0030] The present invention also provides a composite dehumidifying impeller, which is prepared by the method described above.

[0031] This invention utilizes a molecular sieve-polymer composite as the adsorbent matrix and a polymer (resin) as the carrier to prepare a fully adsorbent composite rotor. This significantly avoids the defects caused by "ineffective" glass fiber or ceramic fiber substrates and achieves complementary advantages of the two adsorbent materials. Compared with traditional dehumidification rotors, it avoids the introduction of non-dehumidifying materials such as substrates, increases the adsorption capacity per unit mass of rotor block, and reduces heat loss caused by the heating of the desorption substrate. Using the composite dehumidification rotor of this invention can improve rotor efficiency, avoid the risk of adsorbent shedding, and the strength provided by the molecular sieve can prevent polymer breakage during the adsorption-desorption process. With the molecular sieve-polymer composite as the adsorbent matrix, the molecular sieve ensures dehumidification depth at low humidity, while the organic polymer increases dehumidification capacity at medium and high humidity, effectively ensuring the stability of the rotor's dehumidification performance under different humidity conditions. Attached Figure Description

[0032] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly described below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope of the present invention.

[0033] Figure 1The image shown is of the polymer-molecular sieve extruded honeycomb block product of Example 1 of the present invention.

[0034] Figure 2 A scanning electron microscope image of the polymer-molecular sieve honeycomb block PAA-4A, the product of Example 1 of the present invention, is shown. Detailed Implementation

[0035] As used in this article:

[0036] "Prepared from" is synonymous with "comprising". The terms "comprising", "including", "having", "containing", or any other variations thereof as used herein are intended to cover non-exclusive inclusion. For example, a composition, step, method, article, or apparatus that includes the listed elements is not necessarily limited to those elements, but may include other elements not expressly listed or elements inherent to such composition, step, method, article, or apparatus.

[0037] The conjunction "composed of..." excludes any unspecified elements, steps, or components. If used in a claim, this phrase makes the claim closed, excluding materials other than those described, except for associated conventional impurities. When the phrase "composed of..." appears in a clause of the body of a claim rather than immediately following it, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0038] When a quantity, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pair of any upper or preferred value with any lower or preferred value, regardless of whether the range is disclosed individually. For example, when the range “1–5” is disclosed, the described range should be interpreted as including ranges “1–4”, “1–3”, “1–2”, “1–2 and 4–5”, “1–3 and 5”, etc. When numerical ranges are described herein, unless otherwise stated, the range is intended to include its endpoints and all integers and fractions within that range.

[0039] In these embodiments, unless otherwise specified, the portions and percentages are all by weight.

[0040] "Parts by mass" refers to the basic unit of measurement that expresses the mass ratio of multiple components. One part can represent any unit mass, such as 1g or 2.689g. If we say that component A has "a" parts by mass and component B has "b" parts by mass, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it can mean that the mass of component A is aK and the mass of component B is bK (K is any number representing a multiplier). It is important to understand that, unlike the number of parts by mass, the sum of the mass parts of all components is not limited to 100 parts.

[0041] "And / or" is used to indicate that one or both of the described situations may occur, for example, A and / or B includes (A and B) and (A or B).

[0042] This invention provides a method for preparing a composite dehumidifying rotor and the composite dehumidifying rotor. The preparation method is as follows: S1: Activating and pretreating molecular sieve powder; S2: Adding activated carbon to an acrylic acid solution to remove polymerization inhibitors, and adding an alkaline solution to the supernatant obtained after separation to neutralize and obtain a neutralized solution; S3: Adding the pretreated molecular sieve and crosslinking agent from S1 to the neutralized solution from S2, heating and adding an initiator to stir evenly, controlling the polymerization temperature until a gel-like state is achieved, to obtain a polymer containing molecular sieves; S4: Extruding the polymer containing molecular sieves from S3 into honeycomb blocks; S5: Drying the honeycomb blocks from S4, washing, and then drying them again under vacuum to obtain the final product.

[0043] In this embodiment of the invention, the molecular sieve needs to be dehydrated and activated with sodium hydroxide before use. In step S1, the molecular sieve is dried at 250-550°C, cooled, soaked in a 1-3% alkaline solution for 9-15 hours, washed, and dried. In a preferred embodiment, the molecular sieve is dried at 300°C, cooled, soaked in a 2% alkaline solution for 12 hours, washed, and dried.

[0044] In this embodiment of the invention, the alkaline solution is a NaOH solution.

[0045] In this embodiment of the invention, in step S2, the concentration of the acrylic acid solution is 30-50%; the alkaline solution is NaOH solution; the concentration of the alkaline solution is 10-30%; the mass ratio of the acrylic acid solution to the alkaline solution is (1-3):1; and the neutralization reaction temperature is 15-35℃.

[0046] In a preferred embodiment, in step S2, the concentration of the acrylic acid solution is 40%; the concentration of the alkali solution is 25%; the mass ratio of the acrylic acid solution to the alkali solution is 1:1; and the neutralization reaction temperature is 30°C.

[0047] In this embodiment of the invention, in step S3, the ratio of the molecular sieve to the acrylic acid solution is (5-8):1; the crosslinking agent includes one or more of 1,4-butanediol diacrylate, ethylene glycol dimethacrylate, TAC, butyl acrylate, HEA, HPA, HEMA, HPMA, and MMA; the amount of the crosslinking agent is 0.01-0.03% of the acrylic acid solution; the initiator is an inorganic peroxide; the inorganic peroxide is ammonium persulfate or potassium persulfate; the amount of the initiator is 0.1-0.35% of the acrylic acid solution; the heating is raised to 30-40℃; the polymerization temperature is 50-75℃; and the polymerization reaction time is 2-3 hours.

[0048] In a preferred embodiment, in step S3, the molecular sieve is a type A molecular sieve or a type X molecular sieve powder; the ratio of the molecular sieve to the acrylic acid solution is 6:1; the amount of the crosslinking agent is 0.02% of the acrylic acid solution; the amount of the initiator is 0.2% of the acrylic acid solution; the heating is raised to 35°C; and the polymerization temperature is 65°C.

[0049] An appropriate ratio of molecular sieve to polymer is beneficial for rotor molding and maintaining or improving rotor strength. In composite adsorption materials, the addition of polymer can effectively reduce rotor regeneration temperature, while the strength provided by molecular sieve can significantly prevent polymer breakage defects during adsorption-desorption processes. Strict control of the polymerization reaction within the set temperature is necessary to avoid polymerization rates that are too fast or too slow, which would affect crosslinking density and the network structure within the polymer.

[0050] In this embodiment of the invention, in step S5, the temperature for drying the honeycomb block is 60-80°C; the washing is performed using anhydrous ethanol; and the temperature for the secondary drying under vacuum is 60-80°C.

[0051] In a preferred embodiment, in step S5, the temperature for drying the honeycomb block is 80°C; the temperature for the secondary drying under vacuum is 80°C.

[0052] This invention also provides a composite dehumidifying impeller, which is prepared by the method described above.

[0053] The embodiments of the present invention will be described in detail below with reference to specific examples. However, those skilled in the art will understand that the following examples are for illustrative purposes only and should not be considered as limiting the scope of the invention. Unless otherwise specified in the examples, conventional conditions or conditions recommended by the manufacturer are followed. Reagents or instruments whose manufacturers are not specified are all commercially available products.

[0054] Example 1

[0055] This embodiment provides a method for preparing a composite dehumidifying rotor and the composite dehumidifying rotor itself:

[0056] (1) 500g of 4A molecular sieve raw powder was pretreated and activated. First, the molecular sieve was dried at 250℃. Then, it was soaked in 1.5% sodium hydroxide solution for 9 hours at room temperature to remove impurities and activate the molecular sieve. Finally, it was washed and dried for use.

[0057] (2) Add 10g of activated carbon to 200g of 30% acrylic acid solution to remove the polymerization inhibitor. After centrifugation, transfer the supernatant to a container equipped with a constant pressure titration funnel, thermometer and stirrer. Add 100g of 10% NaOH solution to carry out the neutralization reaction and control the reaction temperature at 20℃.

[0058] (3) Add the molecular sieve pretreated in step (1) and 0.02g of diacrylate-1,4-butanediol ester to the container in step (2), heat to 30°C, add 0.2g of ammonium persulfate and stir evenly, control the polymerization temperature to 50°C and react for 2 hours until a gel is formed;

[0059] (4) Transfer the gel to the material holding area of ​​the hydraulic extrusion molding machine, and adjust the extrusion exit die to extrude the gel into a honeycomb block with a specified through-hole size;

[0060] (5) The honeycomb block obtained in step (4) is dried at 60°C, washed with anhydrous ethanol, and then vacuum dried at 60°C to obtain polymer-molecular sieve honeycomb block (PAA-4A). It is then cut into a specified size of rotor according to requirements to obtain a composite dehumidification rotor with full adsorbent. Figure 1 This is an appearance diagram of the polymer-molecular sieve extruded honeycomb block obtained in this embodiment; Figure 2 This is a scanning electron microscope image of the polymer-molecular sieve honeycomb block PAA-4A.

[0061] Example 2

[0062] This embodiment provides a method for preparing a composite dehumidifying rotor and the composite dehumidifying rotor itself:

[0063] (1) Pre-treat and activate 500g of 13X molecular sieve powder. First, dry the molecular sieve thoroughly at 300℃. Then, soak it in 2% sodium hydroxide solution for 12 hours at room temperature to remove impurities and activate the molecular sieve. Finally, wash and dry it for later use.

[0064] (2) Add 10g of activated carbon to 85g of 40% acrylic acid solution to remove the polymerization inhibitor. After centrifugation, transfer the supernatant to a container equipped with a constant pressure titration funnel, thermometer and stirrer. Add 85g of 25% NaOH solution to carry out the neutralization reaction and control the reaction temperature at 30℃.

[0065] (3) Add the molecular sieve pretreated in step (1) and 0.017g of ethylene glycol dimethacrylate to the container in step (2), heat to 35°C, add 0.17g of ammonium persulfate and stir evenly, control the polymerization temperature to 65°C and react for 2 hours until a gel is formed;

[0066] (4) Transfer the gel to the material holding area of ​​the hydraulic extrusion molding machine, and adjust the extrusion exit die to extrude the gel into a honeycomb block with a specified through-hole size;

[0067] (5) The honeycomb block obtained in step (4) is dried at 80°C, washed with anhydrous ethanol, and then vacuum dried at 80°C to obtain polymer-molecular sieve honeycomb block (PAA-13X). It is then cut into a specified size of rotor according to requirements to obtain a composite dehumidification rotor with full adsorbent.

[0068] Example 3

[0069] This embodiment provides a method for preparing a composite dehumidifying rotor and the composite dehumidifying rotor itself:

[0070] (1) Pre-treat and activate 500g of 5A molecular sieve powder. First, dry the molecular sieve thoroughly at 550℃. Then, soak it in 3% sodium hydroxide solution for 15 hours at room temperature to remove impurities and activate the molecular sieve. Finally, wash and dry it for later use.

[0071] (2) Add 10g of activated carbon to 65g of 50% acrylic acid solution to remove the polymerization inhibitor. After centrifugation, transfer the supernatant to a container equipped with a constant pressure titration funnel, thermometer and stirrer. Add 65g of 30% NaOH solution to carry out the neutralization reaction and control the reaction temperature at 35℃.

[0072] (3) Add the molecular sieve pretreated in step (1) and 0.0195g of 1,4-butanediol diacrylate to the container in step (2), heat to 40°C, add 0.195g of ammonium persulfate and stir evenly, control the polymerization temperature to 75°C and react for 2 hours until a gel is formed.

[0073] (4) Transfer the gel to the material holding area of ​​the hydraulic extrusion molding machine, and adjust the extrusion exit die to extrude the gel into a honeycomb block with a specified through-hole size;

[0074] (5) The honeycomb block obtained in step (4) is dried at 75°C, washed with anhydrous ethanol, and then vacuum dried at 75°C to obtain polymer-molecular sieve honeycomb block (PAA-5A). It is then cut into a specified size of rotor according to requirements to obtain a composite dehumidification rotor with full adsorbent.

[0075] The samples obtained in Examples 1-3 above were analyzed and tested, and the results are as follows:

[0076] 1. Microscopic analysis and testing

[0077] Figure 2 The image shown is a scanning electron microscope image of the polymer-molecular sieve honeycomb block PAA-4A obtained in Example 1. It can be seen that the surface of the composite adsorbent material has many pores. The molecular sieve treated with alkali in the material can play a skeleton role and improve the strength of the rotor. During the polymerization process of the polymer, a large amount of water is present in the product. After drying, the water escapes and leaves a large number of pores on the polymer surface.

[0078] 2. Adsorption performance test

[0079] A portion of the samples prepared in the three examples was taken and dried at a lower regeneration temperature of 100°C for 2 hours. Then, it was placed in an environment of 35°C and 75% humidity. The mass change was tested every 1 hour, and the weight gain rate was calculated, which is the water absorption rate. A certain mass of 4A and 13X molecular sieves were also taken, dried, and tested under the same conditions for comparison. The test results are shown in Table 1. Compared with the pure molecular sieve samples, the polymer of the composite adsorbent greatly enhances the adsorption performance, and the adsorption rate and adsorption capacity are significantly improved.

[0080] Table 1 Comparison of Adsorption Performance

[0081]

[0082] 3. Regeneration performance test

[0083] The saturated adsorbent samples were dried for the same amount of time at different temperatures, and their weight loss rate was calculated to reflect the regeneration performance of the samples. The test results are recorded in Table 2. The weight loss rate of several samples was relatively low at low temperatures, mainly because molecular sieves are not easy to regenerate at low temperatures. At medium temperatures, the polymer in the composite material easily loses water. At this temperature, the composite material loses about 68-71% of the adsorbed water, while the control sample only loses about 45% of the adsorbed water. At high temperatures, all materials tend to complete desorption, which reflects that the composite material has excellent regeneration performance. Based on this, the fully adsorbent composite rotor has broad prospects for the utilization of low-grade heat sources.

[0084] Table 2 Comparison of Regeneration Performance

[0085]

Claims

1. A method for preparing a composite dehumidifying impeller, characterized in that, Includes the following steps: S1: Activation and pretreatment of molecular sieve raw powder; S2: Add activated carbon to the acrylic acid solution to remove the polymerization inhibitor, and add an alkaline solution to the supernatant obtained after separation to carry out a neutralization reaction to obtain a neutralized solution; S3: Add the pretreated molecular sieve and crosslinking agent from S1 to the neutralization solution described in S2, heat up, add the initiator and stir until homogeneous, control the polymerization temperature until a gel-like state is achieved, and obtain a polymer containing molecular sieve. S4: The polymer containing molecular sieves described in S3 is extruded into a honeycomb block; S5: After drying the honeycomb block described in S4, wash it and dry it again under vacuum to obtain the final product.

2. The method for preparing the composite dehumidifying impeller as described in claim 1, characterized in that, In step S1, the activation of the molecular sieve powder refers to drying and sealing the molecular sieve at 250-550℃ and cooling it to room temperature for pretreatment.

3. The method for preparing the composite dehumidifying impeller as described in claim 2, characterized in that, The pretreatment in step S1 refers to soaking the molecular sieve powder in a 1-3% alkaline solution for 9-15 hours after activation, followed by washing and drying.

4. The method for preparing the composite dehumidifying impeller as described in claim 3, characterized in that, In step S1, the alkaline solution is a NaOH solution.

5. The method for preparing the composite dehumidifying impeller as described in claim 1, characterized in that, Step S2 satisfies one or more of the following conditions: a. The concentration of the acrylic acid solution is 30-50%; b. The alkaline solution is a NaOH solution; c. The mass ratio of the acrylic acid solution to the alkaline solution is (1-3):1; d. The neutralization reaction temperature is 15-35℃.

6. The method for preparing the composite dehumidifying impeller as described in claim 5, characterized in that, In step S2, the concentration of the alkaline solution is 10-30%.

7. The method for preparing the composite dehumidifying impeller as described in claim 5, characterized in that, In condition a, the concentration of the acrylic acid solution is 40%. In condition b, the concentration of the alkaline solution is 25%. In condition c, the mass ratio of the acrylic acid solution to the alkaline solution is 1:1; In condition d, the neutralization reaction temperature is 30°C.

8. The method for preparing the composite dehumidifying impeller as described in claim 1, characterized in that, Step S3 satisfies one or more of the following conditions: e. The ratio of the molecular sieve to the acrylic acid solution is (5-8):1; f. The crosslinking agent includes one or more of the following: 1,4-butanediol diacrylate, ethylene glycol dimethacrylate, TAC, butyl acrylate, HEA, HPA, HEMA, HPMA, and MMA; g. The crosslinking agent is used in an amount of 0.01-0.03% of the acrylic acid solution; h. The initiator is an inorganic peroxide; i. The amount of the initiator is 0.1-0.35% of the acrylic acid solution; j. The temperature increase refers to raising the temperature to 30-40℃; k. The polymerization temperature is 50-75℃, and the polymerization reaction time is 2-3h.

9. The method for preparing the composite dehumidifying impeller as described in claim 8, characterized in that, In step S3, the molecular sieve is a type A molecular sieve or a type X molecular sieve powder; The inorganic peroxide is ammonium persulfate or potassium persulfate.

10. The method for preparing the composite dehumidifying impeller as described in claim 8, characterized in that, In condition e, the ratio of the molecular sieve to the acrylic acid solution is 6:1; In condition g, the amount of crosslinking agent is 0.02% of the acrylic acid solution; In condition i, the amount of the initiator is 0.2% of the amount of the acrylic acid solution; In condition j, the temperature increase is to raise the temperature to 35°C; In condition k, the polymerization temperature is 65°C.

11. The method for preparing the composite dehumidifying impeller as described in claim 1, characterized in that, Step S5 satisfies one or more of the following conditions:

1. The drying temperature of the honeycomb block is 60-80℃; m. The washing process uses anhydrous ethanol; n. The temperature for the secondary drying under vacuum is 60-80℃.

12. The method for preparing the composite dehumidifying impeller as described in claim 11, characterized in that, In condition 1, the drying temperature of the honeycomb block is 80°C; In condition n, the temperature of the secondary drying under vacuum is 80°C.

13. A composite dehumidifying impeller, characterized in that, It is prepared by the method of any one of claims 1-12.

Citation Information

Patent Citations

  • Preparation of absorbent resin and MCM-41 molecular sieve composite material

    CN101434676A

  • High static water absorption dehumidifying material and preparation method thereof

    CN110790975A