Flexible switching production device and production method for solution polymerized styrene-butadiene rubber

By using a large-capacity polymerization reactor and a flexible switching production equipment with an efficient heat dissipation system, the problems of untimely heat removal and uneven stirring in the production of solution-polymerized styrene-butadiene rubber have been solved, enabling efficient and stable multi-mode production to meet the needs of a wide viscosity range and multiple grades of products.

CN117920107BActive Publication Date: 2026-11-20ZHONGZHE (ZHEJIANG) POLYMER NEW MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311709029.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-13
Publication Date
2026-11-20
Estimated Expiration
2043-12-13

AI Technical Summary

Technical Problem

Existing solution-polymerized styrene-butadiene rubber (SBR) production equipment suffers from problems such as untimely heat removal and uneven mixing in both continuous and intermittent polymerization modes. This results in low production efficiency, high energy consumption, and unstable product quality, making it impossible to flexibly switch between producing multiple grades of products.

Method used

Design a flexible switching production equipment, including a large-capacity polymerization reactor and a high-efficiency heat dissipation system. It adopts a reactor top condenser, jacketed cooler, internal cooling tube assembly and wide-range agitator, combined with the flexible connection of the feeding system and flash evaporation system to realize the switching between continuous and intermittent polymerization modes, ensuring efficient heat removal and uniform mixing.

Benefits of technology

It improves production efficiency and product quality stability, can adapt to a wide viscosity range under different modes, achieves high output and production of multiple grades of products, and reduces energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117920107B_ABST
    Figure CN117920107B_ABST
Patent Text Reader

Abstract

A flexible switching production device and method of solution polymerized styrene butadiene rubber, the production device comprises a feeding system, a polymerization system, a flash system and a condensation system connected in sequence; the polymerization system comprises at least a first polymerization kettle, a second polymerization kettle and a third polymerization kettle; the production device is flexibly switched between continuous polymerization mode and intermittent polymerization mode: the continuous polymerization mode comprises that the first polymerization kettle, the second polymerization kettle and the third polymerization kettle are connected in series, the first polymerization kettle is connected with the feeding system, and the third polymerization kettle is connected with the flash system; the intermittent polymerization mode comprises that the second polymerization kettle and the third polymerization kettle are connected in parallel, the second polymerization kettle is connected with the feeding system and the flash system respectively, and the third polymerization kettle is connected with the feeding system and the flash system respectively. The present application can realize the flexible switching between the continuous polymerization mode and the intermittent polymerization mode without stopping and cleaning, reduce energy consumption, improve production efficiency and product stability by switching the pipeline connection mode, improving the production capacity and heat removal capacity of the polymerization kettle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of solution-polymerized styrene-butadiene rubber (SBR) preparation technology, and particularly relates to a flexible switching production equipment and production method for solution-polymerized SBR. Background Technology

[0002] Solution-polymerized styrene-butadiene rubber (SBR) is a synthetic rubber prepared by solution polymerization of styrene and butadiene monomers under the action of an initiator. The polymerization process includes continuous polymerization and batch polymerization. Continuous polymerization is generally stable and produces relatively consistent product quality, but it offers limited product variety and flexibility. Batch polymerization, on the other hand, produces a wider range of product grades and offers greater production flexibility. It can be used for solution-polymerized SBR, as well as modified SBR products, low-cis polybutadiene rubber, and styrene-butadiene thermoplastic elastomers (SBCs).

[0003] The polymerization process in solution-polymerized styrene-butadiene rubber (SBR) production is exothermic. The polymerization temperature affects the microstructure of the styrene and butadiene homopolymers, which directly impacts the performance of the rubber product. This is crucial for the polymerization equipment. Existing continuous polymerization processes suffer from drawbacks such as small polymerization reactor volume, lack of internal heat dissipation design, and simple stirring structures. Due to the high viscosity of the materials during polymerization, heat and mass transfer is further hampered. If heat dissipation from the reactants in the reactor is not timely, gel formation and blockage can easily occur, hindering the continuous process and ultimately reducing polymerization capacity and product quality stability while increasing energy consumption. The key technologies for batch polymerization processes are the impurity levels and metering accuracy of the materials. These are closely related to the kinetic characteristics of the polymerization reaction, the concentration of monomers, the properties of the polymer solution, and the size and structure of the polymerization reactor, as well as the stirring method. Existing batch polymerization processes suffer from small polymerization reactor volume, low heat dissipation capacity, untimely and uneven heat dissipation, resulting in low production efficiency and high energy consumption.

[0004] Based on the advantages and disadvantages of continuous polymerization and batch polymerization, existing production processes choose one over the other. The main problem is that they have not solved the heat dissipation problem of the polymerization reactor and the capacity problem of batch polymerization.

[0005] Patent CN113941296A discloses an external circulation reactor and a heat removal method for polymerization reactions. This invention's external circulation heat removal method involves introducing a hexane slurry containing ultra-high molecular weight polyethylene flowing from the bottom of the polymerization reactor into the inner tube of a ring-type condenser in the external circulation system. Then, circulating cooling water is used to exchange heat with the polymerization slurry in the inner tube. The temperature of the polymerization reactor is controlled by interlocking the flow rate of the circulating cooling water with the temperature inside the polymerization reactor. Furthermore, the cooled polymerization slurry can be returned to the polymerization reactor from the upper part to continue the polymerization reaction, thus achieving circulating heat removal from the polymerization reactor. However, this invention uses cooling pipes outside the polymerization reactor, resulting in a large space requirement for the equipment to ensure effective heat removal, without increasing the volume of the polymerization reactor.

[0006] Patent CN214598985U discloses a solution polymerization reactor for styrene-butadiene rubber (SBR) capable of both continuous and batch polymerization. This reactor is equipped with a motor-driven stirrer with stirring blades mounted on its vertical shaft. The reactor is a fluidized bed reactor, and a temperature-controlled water jacket is installed on its outer wall. An external condenser with chilled water inlet and return pipes is mounted on the upper part of the reactor via a support frame. A steam vent at the top of the reactor is connected to a steam inlet pipe, the end of which is connected to the steam inlet at the top of the external condenser. However, this patent only uses a temperature-controlled water jacket on the edge of the reactor, which cannot change the direction and velocity of the cooling water flow, resulting in incomplete heat removal. When switching between continuous and batch polymerization modes, dead zones exist, easily causing accumulation and blockage of the polymer solution. Furthermore, because the viscosity of the reactants changes after mode switching, conventional stirrers cannot adapt to wide viscosity variations, leading to insufficient mixing of the reactants, uneven heat distribution, and unstable polymer quality.

[0007] Therefore, how to provide a solution-polymerized styrene-butadiene rubber production equipment and method that can flexibly switch between continuous polymerization mode and batch polymerization mode, and take advantage of the stability of continuous polymerization production and the flexibility of batch polymerization production to achieve the technical effect of excellent product yield and quality, has become an urgent technical problem to be solved in this field. Summary of the Invention

[0008] To address the deficiencies in the existing technology, the present invention aims to provide a flexible switching production equipment and method for solution-polymerized styrene-butadiene rubber (SBR). This equipment provides timely heat removal when switching production modes, has a stirring structure suitable for a wide viscosity range, thereby ensuring high output in both continuous and batch polymerization modes, stable product quality, and the ability to produce multiple grades of products as needed.

[0009] The first aspect of the present invention provides a flexible switching production equipment for solution-polymerized styrene-butadiene rubber, comprising a feeding system, a polymerization system, a flash evaporation system and a coagulation system connected in sequence;

[0010] The polymerization system includes at least a first polymerization reactor, a second polymerization reactor, and a third polymerization reactor;

[0011] The production equipment can flexibly switch between continuous polymerization mode and intermittent polymerization mode:

[0012] The continuous polymerization mode includes: a first polymerization reactor, a second polymerization reactor, and a third polymerization reactor connected in series, with the first polymerization reactor connected to the feeding system and the third polymerization reactor connected to the flash evaporation system;

[0013] The batch polymerization mode includes: a second polymerization reactor and a third polymerization reactor connected in parallel, the second polymerization reactor being connected to the feed system and the flash evaporation system respectively, and the third polymerization reactor being connected to the feed system and the flash evaporation system respectively.

[0014] Batch polymerization processes are characterized by high production flexibility and adaptability to various product types; while continuous processes are characterized by stable product quality, high production efficiency, low energy consumption, and easy control of the reaction process. Compared with batch processes, continuous processes have lower material and energy consumption, higher production efficiency, and more stable product quality, representing the development direction of solution polymerization of lithium-based polymers such as styrene-butadiene rubber. This invention understands the characteristics of both polymerization processes and utilizes their advantages to obtain production equipment that is flexible in switching and highly adaptable to different production environments.

[0015] Preferably, the feeding system includes a butadiene refining unit, an isoprene refining unit, a styrene refining unit, and a solvent refining unit; and optionally includes a continuous polymerization aid unit for continuous polymerization mode and a batch polymerization aid unit for batch polymerization mode.

[0016] By setting up styrene refining, butadiene refining, and solvent refining units, the oxygen content and initiator poison content of the system can be controlled at low levels. This helps to avoid the risk of initiator deactivation during production, recycling, and production switchover, ensuring low gel content and high conversion rate.

[0017] Preferably, the continuous polymerization aid unit includes at least one of the following: a continuous polymerization catalyst feed port, a continuous polymerization activator feed port, a continuous polymerization scale inhibitor feed port, a continuous polymerization coupling agent feed port, and a continuous polymerization modifier feed port;

[0018] The batch polymerization aid unit includes at least one of the following: batch polymerization catalyst feed port, batch polymerization activator feed port, batch polymerization front-end modifier feed port, batch polymerization back-end modifier feed port, and batch polymerization coupling agent feed port.

[0019] Based on the differences in the types and addition methods of materials used in continuous polymerization and batch polymerization processes, this invention has adjusted and modified the production equipment. The existing feeding systems that are adapted to continuous / batch polymerization processes, especially the auxiliary agent unit, have been arranged and integrated, thereby providing basic material support for flexible switching.

[0020] The batch polymerization aid unit utilizes the chemical reactions of monomers, initiators, and catalysts within the polymerization reactor to link monomer molecules together and form long-chain macromolecules. Its operation involves evacuating the polymerization reactor to a vacuum state, adding the monomers and initiators according to a specific ratio, and controlling parameters such as temperature and pressure to carry out the polymerization reaction and obtain the polymer product. Simultaneously, product quality can be controlled by factors such as polymer particle size and particle size distribution.

[0021] Preferably, in the continuous polymerization mode, the feeding system is connected to the bottom inlet A1 of the first polymerization reactor after passing through the mixer, the top outlet A2 of the first polymerization reactor is connected to the bottom inlet B1 of the second polymerization reactor, the top outlet B2 of the second polymerization reactor is connected to the bottom inlet C1 of the third polymerization reactor, and the top outlet C2 of the third polymerization reactor is connected to the flash evaporation system.

[0022] Preferably, in the batch polymerization mode, the solvent purification unit is connected to the bottom feed port B1 of the second polymerization reactor and the bottom feed port C1 of the third polymerization reactor, respectively;

[0023] The isoprene refining unit and the styrene refining unit are respectively connected to the top feed port B3 of the second polymerization reactor and the top feed port C3 of the third polymerization reactor;

[0024] The butadiene refining unit is connected to the bottom feed port B1 and top feed port B3 of the second polymerization reactor, and to the bottom feed port C1 and top feed port C3 of the third polymerization reactor.

[0025] Each feed port in the batch polymerization aid unit is connected to the top feed port B3 of the second polymerization reactor and the top feed port C3 of the third polymerization reactor, respectively.

[0026] Furthermore, the bottom outlet B4 of the second polymerization reactor and the bottom outlet C4 of the third polymerization reactor are respectively connected to the flash evaporation system.

[0027] The aforementioned connection methods enable the first, second, and third polymerization reactors to be connected in series for continuous polymerization processes, while the larger second and third polymerization reactors can be connected in parallel for batch polymerization processes. Through the overall connection layout and switching of the feeding system, polymerization system, flash evaporation system, and condensation system, this invention achieves flexible switching between continuous and batch polymerization modes, ensuring both output and product quality. Furthermore, the number of polymerization reactors in both modes is not limited to the above design and can be increased or decreased based on capacity requirements and energy balance.

[0028] Preferably, the volumes of the second and third polymerization reactors are 1.5-2.5 times the volume of the first polymerization reactor, and the second and third polymerization reactors are respectively equipped with a heat dissipation system, which includes a jacketed cooler and several internal cooling pipe groups;

[0029] The jacketed cooler includes a cooling water jacket covering the outer wall of the polymerization reactor, a cooling water inlet at the bottom of the cooling water jacket, and several cooling water outlets at the top of the cooling water jacket.

[0030] The internal cooling tube assembly includes multiple internal cooling vertical tubes extending axially along the polymerization reactor, and the surface roughness Ra of the internal cooling vertical tubes is ≤0.1μm.

[0031] Traditional polymerization reactors typically control polymerization temperature using a jacket and internal cooling pipes with cooling water. This method is limited by the low thermal conductivity of the polymer on the reactor wall and polymer adhesion to the wall, and can only remove about 10% of the polymerization heat within a specified time. Using low-temperature media (such as chilled brine or liquid ammonia) to increase heat transfer can easily cause polymer deposition on the reactor wall; external circulation for heat removal increases equipment investment, leads to pipe and heat exchanger blockages, increases energy consumption due to large-volume polymer transport, and is inconvenient to operate; natural evaporation and reflux for heat removal is also ineffective due to its slow evaporation rate. Furthermore, existing polymerization reactors use multiple tube bundles or multi-layered coiled tubes as internal cooling components. When these cooling media pass through these small-diameter tube bundles or multi-layered coiled tubes, the presence of numerous gaps between the tubes causes polymer stagnation or accumulation in dead flow zones, easily leading to polymer buildup and blockage.

[0032] This invention employs a vertically arranged internal cooling tube assembly with a specific distribution. It contains at least four connecting channels, which alter the flow direction and velocity of the cooling medium to improve heat transfer efficiency. The internal cooling tube assembly is connected to the inlet and outlet of the internal cooling medium. The internal cooling tubes have a simple shape, with either a flat or curved surface, and can be machined to a high-gloss finish, eliminating dead zones. The shape and geometry of the internal cooling tubes, their arrangement, position, and number within the reactor can be determined according to heat and mass transfer requirements, and coordinated with the stirring impeller to effectively control the temperature and its distribution within the reactor. Furthermore, a cooling water jacket is provided outside the polymerization reactor to further aid in rapid heat dissipation, improve reaction uniformity, and stabilize polymer quality.

[0033] Specifically, the volumes of the second and third polymerization reactors are preferably greater than 70 m³. 3 This volume is much larger than that of commonly used polymerization reactors, such as the first polymerization reactor, whose volume is typically 30-40 m³. 3 .

[0034] Due to the increased volume, the production capacity of the batch polymerization mode increases significantly, but it also places extremely high demands on the heat dissipation effect. This invention provides a heat dissipation system for the large-capacity second and third polymerization reactors, including but not limited to a reactor top condenser, a jacketed cooler, several internal cooling pipe assemblies, and a heat dissipation agitator.

[0035] The reactor top condenser condenses and cools the gaseous phase during the polymerization reaction, returning it to the polymerization reactor. This facilitates timely and uniform removal of polymerization heat, reducing the chilled water volume and heat removal pressure of the jacketed cooler, and decreasing energy consumption. The jacketed cooler includes a cooling water jacket covering the outer wall of the polymerization reactor, a cooling water inlet at the bottom of the jacket, and several cooling water outlets at the top of the jacket. Preferably, guide ribs or flow dividers are provided on the inner wall of the jacketed cooler to ensure uniform dispersion of cooling water within the jacket, fully covering the polymerization reactor wall and effectively removing heat from the reactor. Multiple outlets can be evenly distributed in the upper part of the jacket, allowing the heated water to be discharged promptly, increasing the cooling water circulation rate.

[0036] The internal cooling pipe assembly includes multiple internal cooling vertical pipes extending axially along the polymerization reactor. These internal cooling pipe assemblies are arranged along the inner wall of the reactor and supported and fixed to the inner wall by the internal cooling pipes. Each internal cooling pipe assembly has at least four connecting channels, each connecting to a separate internal cooling vertical pipe. These channels alter the flow direction and velocity of the cooling medium to improve heat transfer efficiency. Each internal cooling pipe assembly is connected to the inlet and outlet of the internal cooling medium. The internal cooling vertical pipes have a simple shape, with either a flat or curved surface, and are machined to a smooth surface with no dead zones. The surface roughness Ra of the internal cooling vertical pipes is ≤0.1μm, preferably Ra≤0.08μm.

[0037] Preferably, the heat dissipation system further includes heat dissipation agitators arranged axially along the interior of the second and third polymerization reactors, respectively. Each heat dissipation agitator includes a rotating shaft and a wide-width stirring paddle connected to the rotating shaft. The rotating shaft and the wide-width stirring paddle have a cooling water passage communicating with each other. The width of the wide-width stirring paddle accounts for 60-90% of the internal diameter of the polymerization reactor, and its height accounts for 60-90% of the internal height of the polymerization reactor.

[0038] This invention includes a heat-dissipating agitator in each polymerization reactor, which can be one of a spiral agitator, a multi-bladed composite agitator, or a sickle-shaped agitator. Due to the significantly increased volume of the second and third polymerization reactors, the heat-dissipating agitators require further design.

[0039] The wide-width agitator used in this invention has a large width-to-inner-diameter ratio, resulting in high heat transfer capacity for high-viscosity fluids. Its large blade height also enhances its adaptability to liquid surface fluctuations. The wide-width agitator, in conjunction with a variable-speed motor, utilizes high speed for low viscosity and low speed for high viscosity, enabling the heat-dissipating agitator to achieve the required stirring and heat dissipation effects in different polymerization modes. Preferably, the wide-width agitator employs a trapezoidal frame, i.e., a non-planar continuous plate-shaped agitator, with several parallel openings near the rotation axis. This ensures wide-width stirring without significantly increasing stirring resistance or liquid vortex, resulting in stable and safe production. More preferably, disturbance plates are added to the openings, and these plates are asymmetrically arranged on both sides of the rotation axis. For example, vertical disturbance plates are placed in one opening, while horizontal disturbance plates are formed in the other, thereby achieving better stirring of the liquid inside the vessel. Based on this asymmetrical arrangement design, the angle of the disturbance plates on each side can be designed according to the stirring and heat dissipation requirements. The wide-width stirring impeller, especially the agitator, preferably has a surface roughness Ra≤0.1μm to prevent clogging of the gaps and facilitate subsequent cleaning.

[0040] Compared to existing polymerization reactors that use multiple tube bundles or multi-layer disc tubes as internal cooling components, which have a large number of gaps between tubes, causing the adhesive to stagnate or accumulate in the flow dead zone, easily leading to adhesive accumulation and blockage, the composite heat dissipation system of this invention can not only improve the heat dissipation effect, but also avoid problems such as accumulation and blockage.

[0041] Preferably, the flash evaporation system includes a flash tank, a solvent condenser, a flash solution condensate tank, and a flash solvent molecular sieve. The liquid phase outlet of the flash tank is connected to a condensation unit, and the gas phase outlet is sequentially connected to the solvent condenser, the flash solution condensate tank, and the flash solvent molecular sieve, so that the cooled and refined solvent is returned to the feeding system.

[0042] Flash evaporation technology utilizes the different boiling points of mixtures and the principle of gas-liquid equilibrium for separation. It involves heating the mixture to its boiling point, then passing it through a flash evaporator to vaporize it, separating the liquid and gas. Flash evaporation technology offers advantages such as high efficiency, flexibility, and low energy consumption. It can rapidly separate liquid mixtures, improving production efficiency and reducing costs. It is suitable for mixtures of various compounds, requires relatively little energy, and can therefore be used for extended periods in industrial environments without excessive energy consumption. It is widely used in petroleum processing, chemical industries, and other fields.

[0043] Based on the aforementioned flexible switching production equipment for solution-polymerized styrene-butadiene rubber (SBR), a second aspect of the present invention provides a flexible switching production method for SBR, wherein the production method flexibly switches between continuous polymerization mode and batch polymerization mode by switching the connection mode of the feeding system, polymerization system, and flash evaporation system; comprising:

[0044] (1) Connect the first polymerization reactor, the second polymerization reactor and the third polymerization reactor in series. The first polymerization reactor is connected to the feeding system and the third polymerization reactor is connected to the flash evaporation system to enter the continuous polymerization mode.

[0045] (2) Connect the second polymerization reactor and the third polymerization reactor in parallel. The second polymerization reactor is connected to the feeding system and the flash evaporation system respectively, and the third polymerization reactor is connected to the feeding system and the flash evaporation system respectively, and enter the batch polymerization mode.

[0046] Preferably, in the batch polymerization mode, the refined solvent is fed into the second polymerization reactor through the bottom inlet B1 and the third polymerization reactor through the bottom inlet C1; the refined isoprene and refined styrene are fed into the second polymerization reactor through the top inlet B3 and the third polymerization reactor through the top inlet C3; the refined butadiene is fed into the second polymerization reactor through the bottom inlet B1 and the top inlet B3, and into the third polymerization reactor through the bottom inlet C1 and the top inlet C3; the batch polymerization auxiliary is fed into the second polymerization reactor through the top inlet B3 and the top inlet C3.

[0047] In this invention, a segmented feeding method is used for refined butadiene in a batch polymerization process. The first segment involves adding the first group of butadiene from the bottom feed inlet of the polymerization reactor, followed by the second segment from the top feed inlet. To effectively adjust the styrene-bound styrene content and maintain a constant mixed monomer concentration, the butadiene concentration is artificially controlled to remain at a very low level, promoting K... BS [B - [S]≈K BB [B - The challenge lies in maintaining a constant [B] / [S] ratio, requiring the addition of different amounts of butadiene in different reaction zones based on the conversion rate of [S]. This necessitates highly automated facilities to accurately adjust the butadiene addition. This invention employs a precise control method using dual mass flow meters and regulating valves, with an APC control system ensuring the accuracy of segmented butadiene addition. Structurally, the segmented feeding method can produce completely random S-SBR, with almost no styrene repeating units greater than 3 in the molecular chain. This indicates that controlling the monomer polymerization rate by adjusting the monomer concentration is an effective means to prevent the formation of excessively long polystyrene segments. Analysis of the vulcanizate properties shows that the S-SBR prepared by the segmented feeding method has lower hysteresis loss, 20% lower than the uM method and 30% lower than the STA method, while other properties are essentially the same.

[0048] The advantages of this invention are as follows:

[0049] (1) The production equipment of the present invention achieves flexible switching between continuous polymerization mode and batch polymerization mode of solution-polymerized styrene-butadiene rubber by switching the connection mode of feeding system, polymerization system and flash evaporation system, thereby improving production capacity while ensuring product quality and being compatible with the production of multiple grades of products.

[0050] (2) This invention uses a large-capacity polymerization reactor to compensate for the insufficient production capacity of the batch polymerization process, and is equipped with a high-efficiency heat dissipation system to ensure good heat removal effect while maintaining high production capacity, thereby ensuring product quality. The heat dissipation combination of a top vapor phase condenser, a jacketed cooler, an internal cooling tube group with multiple internal cooling vertical tubes, and a high-performance heat dissipation agitator significantly improves heat transfer efficiency and heat removal rate, effectively controls the temperature inside the reactor when switching polymerization modes, avoids accumulation and blockage of the glue, improves reaction uniformity, and stabilizes polymer quality.

[0051] (3) The heat dissipation stirrer in the polymerization reactor of the present invention has a wide range of applicable viscosity. It can make the materials and temperature distribution of various viscosity ranges uniform in polymerization reactors under different polymerization modes, ensuring the uniformity of the product. Moreover, the cooling water passage connected to its rotating shaft and the wide-width stirring paddle can dissipate heat from the inside of the material, effectively relieving the heat dissipation pressure of the jacket cooler and internal cooling pipe group distributed around it, and improving the overall heat dissipation effect of the production equipment. Attached Figure Description

[0052] The above and other objects, features, and advantages of exemplary embodiments of the present disclosure will become readily apparent upon reading the following detailed description with reference to the accompanying drawings. In the drawings, several embodiments of the present disclosure are illustrated by way of example and not limitation, and like or corresponding reference numerals denote like or corresponding parts, wherein:

[0053] Figure 1 This is a schematic diagram of the flexible switching production equipment of the present invention;

[0054] Figure 2 This is a top view of the internal cooling pipe assembly of the present invention;

[0055] Figure 3 This is a front view of the internal cooling pipe assembly of the present invention;

[0056] Figure 4 This is a schematic diagram of the heat dissipation system of the present invention.

[0057] Explanation of reference numerals in the attached figures: 1. Butadiene refining unit; 11. Butadiene water washing tower; 12. Butadiene dehydration tower; 13. Butadiene de-heavy tower; 14, 15. Butadiene oil molecular sieve; 16. Refined butadiene and refined solvent mixer; 2. Isoprene refining unit; 21. Isoprene water washing tower; 22. Isoprene dehydration tower; 23. Isoprene dehydration tower; 24, 25. Isoprene and solvent mixture molecular sieve; 26. Refined isoprene and refined solvent mixer; 3. Solvent refining unit; 31. Solvent water washing tower; 32. Solvent de-heavy tower. 33. Solvent deweighting tower 1, 34. Solvent deweighting tower 2, 35. Solvent residue tower, 4. Styrene refining unit, 41, 42. Styrene-alumina refining bed, 43. Styrene and refined solvent mixer, 5. Polymerization system, 511. Batch polymerization catalyst feed port, 512. Batch polymerization activator feed port, 513. Batch polymerization front-end modifier feed port, 514. Batch polymerization back-end modifier feed port, 515. Batch polymerization coupling agent feed port, 516. Continuous polymerization catalyst feed port, 517. Continuous polymerization 518. Activator feed port; 519. Continuous polymerization scale inhibitor feed port; 520. Continuous polymerization coupling agent feed port; 521. Continuous polymerization modifier feed port; 522. Second polymerization reactor top condenser; 523. Third polymerization reactor top condenser; 524. First polymerization reactor; 525. Second polymerization reactor; 526. Third polymerization reactor; 527. Static mixer; 528. Preheater; 529. Precooler; 6. Flash evaporation system; 61. Flash tank; 62. Solvent condenser; 63. Flash solvent condensate tank; 64. 65. Flash solvent molecular sieve; 7. Condensation system; 71. Final condensation vessel; 72. Steam ejector; 73. Intermediate condensation vessel; 74. First condensation vessel; 75. Waste heat utilization system; 76. Condensation cooler; 77. Tail gas condenser; 78. Tail gas compressor; 79. Oil-water separation tank; 8. Cooling water jacket; 81. Water inlet; 82. Water outlet; 9. Internal cooling pipe assembly; 91. Internal cooling vertical pipe; 92. Cooling water inlet; 93. Cooling water outlet; 10. Radiator agitator; 101. Rotating shaft; 102. Wide-width agitator. Detailed Implementation

[0058] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described in further detail below.

[0059] like Figure 1 The flexible switching production equipment for solution-polymerized styrene-butadiene rubber shown includes a feeding system, a polymerization system 5, a flash evaporation system 6 and a condensation system 7 connected in sequence.

[0060] (1) A feeding system, including butadiene refining unit 1, isoprene refining unit 2, solvent refining unit 3 and styrene refining unit 4, as well as a continuous polymerization aid unit for continuous polymerization mode and a batch polymerization aid unit for batch polymerization mode.

[0061] The butadiene refining unit 1 includes, in the following order: butadiene water washing tower 11, butadiene dehydration tower 12, butadiene deweighting tower 13, refined butadiene and refined solvent mixer 16, and butadiene oil molecular sieve (14, 15).

[0062] The isoprene refining unit 2 includes, in the following order: isoprene washing tower 21, isoprene dehydration tower 22, isoprene de-weighting tower 23, refined isoprene and refined solvent mixer 26, and isoprene and solvent mixture molecular sieve (24, 25).

[0063] The solvent refining unit 3 includes, in the following order: solvent washing tower 31, solvent dehydration tower 32, solvent de-weighting tower 1 33, solvent de-weighting tower 2 34, and solvent residue tower 35.

[0064] The styrene refining unit 4 includes, in the order of connection, a styrene-alumina refining bed (41, 42) and a styrene and solvent mixer 43;

[0065] The continuous polymerization aid unit includes a continuous polymerization catalyst feed port 516, a continuous polymerization activator feed port 517, a continuous polymerization scale inhibitor feed port 518, a continuous polymerization coupling agent feed port 519, and a continuous polymerization modifier feed port 520.

[0066] The batch polymerization aid unit includes a batch polymerization catalyst feed port 511, a batch polymerization activator feed port 512, a batch polymerization front-end modifier feed port 513, a batch polymerization back-end modifier feed port 514, and a batch polymerization coupling agent feed port 515.

[0067] (2) The polymerization system 5 includes a polymerization reactor, wherein the polymerization reactor comprises, in sequence, a first polymerization reactor 523, a second polymerization reactor 524, and a third polymerization reactor 525. The volumes of the second polymerization reactor 524 and the third polymerization reactor 525 are 1.5-2.5 times the volume of the first polymerization reactor 523, respectively. The second polymerization reactor 524 and the third polymerization reactor 525 each have a heat dissipation system, wherein the heat dissipation system includes a jacketed cooler and a plurality of internal cooling pipe groups 9, preferably 2-6 groups of internal cooling pipe groups 9.

[0068] The jacketed cooler includes a cooling water jacket 8 covering the outer wall of the polymerization reactor, a cooling water inlet 81 at the bottom of the cooling water jacket 8, a plurality of cooling water outlets 82 at the top of the cooling water jacket, and a plurality of optional thermometers and level gauges.

[0069] The internal cooling pipe group 9 includes multiple internal cooling vertical pipes 91 extending along the axial direction of the polymerization reactor. For example, each internal cooling pipe group 9 has 24 internal cooling vertical pipes 91. When three groups are set up, a total of 72 internal cooling vertical pipes 91 are used. Figure 2 and Figure 3 The surface roughness Ra of the internal cooling riser 91 is ≤0.1μm. The internal cooling risers 91 in each group of internal cooling pipes are connected sequentially. The flow direction and velocity of the cooling medium can be changed multiple times within each group of internal cooling pipes 9 to improve heat transfer efficiency. Each group of internal cooling pipes 9 has a cooling water inlet 92 and a cooling water outlet 93, as well as several optional thermometers and level gauges.

[0070] The heat dissipation system also includes heat dissipation agitators 10 respectively arranged along the internal axial direction of the second polymerization reactor 524 and the third polymerization reactor 525. The heat dissipation agitator includes a rotating shaft 101 and a wide-width agitator 102 connected to the rotating shaft. The rotating shaft 101 and the wide-width agitator 102 have a cooling water passage communicating with each other. The width of the wide-width agitator 102 accounts for 60-90% of the internal diameter of the polymerization reactor, and the height accounts for 60-90% of the internal height of the polymerization reactor.

[0071] In the preparation of solution-polymerized styrene-butadiene rubber (SBR), especially in batch polymerization mode, the viscosity of the reactant system varies greatly during polymerization. At the beginning of polymerization, the viscosity of the system is close to that of the solvent, generally less than tens of millipascals per second (mPa·s), while in the later stages of polymerization, the viscosity can rise to thousands, tens of thousands, or even hundreds of thousands of mPa·s. Generally, agitators are mainly divided into two categories: those for low viscosity and those for high viscosity. Agitators that can maintain high efficiency in both mixing and heat transfer over such a wide viscosity range are even rarer. Furthermore, in batch polymerization, the liquid level in the reactor is generally low at the beginning of polymerization, gradually rising as polymerization progresses. Maintaining high mixing efficiency with the agitator under such significant fluctuations in liquid level is also a challenge. Traditional polymerization reactors use simple multi-layer paddle agitators. Besides heat release through coils and jackets, a large portion of the polymerization heat is released through the evaporation of solvent or monomer via a condenser at the top of the reactor. However, if the viscosity of the material in the reactor is very high, mixing it with the low-viscosity solvent or monomer flowing down from the condenser is also very difficult. In such cases, a simple agitator alone cannot achieve good results. Therefore, this invention designs a special type of heat-dissipating agitator adaptable to a wide viscosity range. Key features include a wide-width agitator with wide and long blades. The wide-width agitator has a wide applicable viscosity range; due to its large diameter-to-bottle diameter ratio, it has high heat transfer capacity for high-viscosity fluids; furthermore, due to its long blades, it has strong adaptability to liquid surface fluctuations. (See appendix.) Figure 4 The wide-width stirring paddle, combined with a variable-speed motor (constant power output type), allows for high speed at low viscosity and low speed at high viscosity. In conjunction with its internal cooling water passage, internal cooling pipe assembly, jacketed cooler, and top condenser, it can achieve excellent stirring and heat dissipation effects.

[0072] The aforementioned polymerization reactor is designed to connect to the feed inlets of each material in the feeding system. The opening and closing of the feed inlets is switched according to the selection of continuous or batch polymerization mode. Specifically:

[0073] (2.1) In the continuous polymerization mode, the feeding system is connected to the bottom inlet A1 of the first polymerization reactor 523 after passing through the mixer. The top outlet A2 of the first polymerization reactor 523 is connected to the bottom inlet B1 of the second polymerization reactor 524. The top outlet B2 of the second polymerization reactor 524 is connected to the bottom inlet C1 of the third polymerization reactor 525. The top outlet C2 of the third polymerization reactor 525 is connected to the flash evaporation system 6.

[0074] (2.2) In the batch polymerization mode, the solvent purification unit 3 is connected to the bottom feed port B1 of the second polymerization reactor 524 and the bottom feed port C1 of the third polymerization reactor 525, respectively;

[0075] The isoprene refining unit 2 and the styrene refining unit 4 are respectively connected to the top feed port B3 of the second polymerization reactor 524 and the top feed port C3 of the third polymerization reactor 525;

[0076] The butadiene refining unit 1 is connected to the bottom feed port B1 and the top feed port B3 of the second polymerization reactor 524, and to the bottom feed port C1 and the top feed port C3 of the third polymerization reactor 525.

[0077] Each feed port in the batch polymerization aid unit is connected to the top feed port B3 of the second polymerization reactor 524 and the top feed port C3 of the third polymerization reactor 525, respectively.

[0078] Furthermore, the bottom outlet B4 of the second polymerization reactor 524 and the bottom outlet C4 of the third polymerization reactor 525 are respectively connected to the flash evaporation system 6.

[0079] (3) Flash evaporation system 6 includes flash tank 61, solvent condenser 62, flash solution condensate tank 63 and flash solvent molecular sieve (64, 65). The liquid phase outlet of flash tank 61 is connected to the condensation unit, and the gas phase outlet is connected in sequence to solvent condenser 62, flash solution condensate tank 63 and flash solvent molecular sieve (64, 65) to return the cooled and refined solvent to the feed system.

[0080] (4) The condensation system 7 includes a condensation starter 74, a condensation intermediate 73, a condensation finisher 71, a solvent recovery system, and a reflux system connected in sequence. The condensation starter 74 is connected to the liquid phase outlet of the flash tank 61, and the oil-water separation tank 79 is connected to the solvent refining unit 3. The solvent recovery system includes a recovery pipeline connected to the top outlet of the condensation starter 74. After the recovery pipeline, the waste heat utilization system 75, the condensation cooler 76, and the oil-water separation tank 79 are connected in sequence. The tail gas of the oil-water separation tank 79 is returned to the condensation cooler 76 after passing through the tail gas condenser 77 and the tail gas compressor 78. The liquid phase of the oil-water separation tank 79 is returned to the solvent refining unit 3. A steam ejector 72 is also included at the top outlet of the condensation finisher 71 to smoothly return the high-temperature gas phase to the condensation starter 74.

[0081] This solution-polymerized styrene-butadiene rubber (SBR) production equipment can flexibly switch between continuous polymerization and batch polymerization modes, thus providing a flexible switching production method for SBR. This is achieved by switching the connection methods of the feeding system, polymerization system 5, and flash evaporation system 6, allowing for flexible switching between continuous and batch polymerization modes; including:

[0082] 1. Enter continuous aggregation mode

[0083] (1) The refined solvent from the solvent refining unit 3 and the flash evaporation system, after being preheated or precooled, is mixed with refined butadiene oil from the butadiene refining unit 1, refined benzene oil from the styrene refining unit 4, and refined isoprene from the isoprene refining unit 2. After adding scale inhibitor and activator, it enters the static mixer 526, and then the catalyst is added and enters the static mixer 527.

[0084] (2) The first polymerization reactor 523, the second polymerization reactor 524 and the third polymerization reactor 525 are connected in series. The static mixer 527 is connected to the bottom feed port A1 of the first polymerization reactor 523 and the top discharge port A2 discharges into the bottom feed port B1 of the second polymerization reactor 524. The polymerization is further carried out in the second polymerization reactor 524. The discharge port B2 of the second polymerization reactor 524 discharges into the bottom feed port C1 of the third polymerization reactor 525. The polymerization is further carried out in the third polymerization reactor 525. Then the discharge port C2 of the third polymerization reactor 525 discharges into the flash evaporation system 6.

[0085] In addition, when producing branched grades, coupling agents and modifiers can be added to the bottom feed inlet B1 of the second polymerization reactor 524 and the bottom feed inlet C1 of the third polymerization reactor 525, respectively.

[0086] (3) After the adhesive solution enters the flash tank 61, flash evaporation occurs, and part of the solvent in the adhesive solution vaporizes and enters the flash solvent condenser 62 to condense into a liquid phase. Then, it enters the flash solvent condensate tank 63 and passes through the flash solvent molecular sieves (64, 65) to remove impurities from the solvent. The liquid is then returned to the feeding system. The flash-evaporated adhesive solution is sent to the coagulation unit, where the solvent in the coagulation kettles connected in series is removed. The removed solvent is refined and recycled. The coagulated rubber particles are sent to the post-processing unit for dehydration, drying, briquetting, and packaging before being shipped as rubber products.

[0087] The continuous polymerization of solution-polymerized styrene-butadiene rubber generally includes the following steps:

[0088] 1) Control the feed temperature at 50-65℃, and set the feed rates for butadiene, styrene, solvent, catalyst, activator, and scale inhibitor. For example, the feed rate for butadiene is 65-85 phm, the feed rate for styrene is 20-30 phm, the feed rate for solvent is 450-550 phm, the feed rate for catalyst is 0.02-0.03 phm, the molar ratio of activator to catalyst is 4.1-4.5, and the feed rate for scale inhibitor is 0.1-0.3 phm.

[0089] 2) The first polymerization reactor is maintained at 70-80℃ and 0.5-0.7 MPa to ensure a monomer conversion rate of over 99%, preferably 99-99.8%. The second and third polymerization reactors are also individually temperature and pressure controlled: the second reactor is maintained at 60-70℃ and 0.4-0.6 MPa, and the third reactor is maintained at 60-70℃ and 0.4-0.5 MPa. When producing branched grades, coupling agents and modifiers are added to the bottom inlets of both the second and third polymerization reactors.

[0090] 2. Enter intermittent aggregation mode

[0091] The first polymerization reactor 523 is temporarily suspended. The second polymerization reactor 524 and the third polymerization reactor 525 are connected in parallel. The second polymerization reactor 524 is connected to both the feeding system and the flash evaporation system 6. The third polymerization reactor 525 is connected to both the feeding system and the flash evaporation system 6.

[0092] The refined solvent from solvent refining unit 3 and the flash evaporation system, after passing through preheater 528 and / or precooler 529, merges with a portion of refined butadiene from butadiene refining unit 1 and enters the polymerization reactor from the bottom of the second polymerization reactor 524 and the third polymerization reactor 525, respectively. Another portion of refined butadiene from butadiene refining unit 1, refined styrene from styrene refining unit 4, and refined isoprene from isoprene refining unit 2 enter the polymerization reactor from the top of the second polymerization reactor 524 and the third polymerization reactor 525, respectively. Through batch polymerization catalyst feed port 511, batch polymerization activator feed port 512, batch polymerization front-end modifier feed port 513, batch polymerization back-end modifier feed port 514, and batch polymerization coupling agent feed port 515, under specific feeding procedures and operating conditions, the activator and front-end modifier are added quantitatively first, followed by the catalyst, and finally the back-end modifier and coupling agent. The materials react in the polymerization reactor, and after the reaction is complete, a gel is obtained.

[0093] During batch polymerization, the polymerization reactors are not operated at full capacity. The gaseous phase from the top of the second polymerization reactor 524 and the third polymerization reactor 525 enters the top condenser 521 of the second polymerization reactor and the top condenser 522 of the third polymerization reactor, respectively. The gaseous material is condensed into a liquid phase in the condenser and then returns to the polymerization reactor to cool it down. The polymerized rubber solution is discharged from the bottom of the second polymerization reactor 524 and the third polymerization reactor 525 to the flash evaporation system 6. After entering the flash evaporation tank 61, the rubber solution undergoes flash evaporation, and part of the solvent in the rubber solution vaporizes and enters the flash solvent condenser 62 to condense into a liquid phase. Then, it enters the flash solvent condensate tank 63 and then passes through the flash solvent molecular sieves (64, 65) to remove impurities from the solvent. It then returns to the feed system. The flash-evaporated rubber solution is sent to the coagulation unit, where the solvent is removed from the rubber solution in the coagulation tank. The removed solvent is purified and recycled. The coagulated rubber granules are sent to the post-processing unit for dehydration, drying, briquetting, and packaging before being shipped as rubber products.

[0094] The batch polymerization mode of solution-polymerized styrene-butadiene rubber generally includes the following steps:

[0095] 1) Add solvent to the second polymerization reactor 524 and the third polymerization reactor 525;

[0096] 2) After the solvent feeding begins, the solvent preheater and precooler start controlling the solvent feed temperature so that the temperature inside the second polymerization reactor 524 and the third polymerization reactor 525 reaches the polymerization initiation temperature Ti, approximately 20±2℃; preferably, the lowest temperature value of at least three temperature detectors inside the polymerization reactor is measured and read as Ti. During the solvent feeding period, the feed temperature of the solvent preheater and precooler is estimated and controlled based on the polymerization reactor temperature-time curve so that the temperature inside the polymerization reactor reaches the initiation temperature Ti after the solvent, butadiene, styrene, activator and front-end modifier are fed.

[0097] 3) When the amount of solvent added reaches the starting value of 12-14t, start the heat dissipation agitator of the polymerization reactor, and continue to feed the solvent until the set value is reached;

[0098] 4) After stirring is started, add butadiene, styrene, activator and front-end modifier;

[0099] 5) Add the catalyst to the catalyst feeding tank according to the set amount; add the downstream modifier to the downstream modifier feeding tank according to the set amount;

[0100] 6) Butadiene, styrene, activator and front-end modifier feeding is completed; among them, butadiene, styrene, activator and front-end modifier feeding is completed before solvent feeding is completed;

[0101] 7) After the material feeding in step 6) is completed, estimate the volume of material in the polymerization reactor based on the liquid level displayed by the level gauge, calculate the difference between the value and the value measured by the flow meter, and the deviation must be within the allowable range; check and monitor whether the temperature inside the polymerization reactor is within the range of 20±2℃ of the initiation temperature.

[0102] 8) If the inspection finds no problems, the catalyst will be added to the polymerization reactor, and the polymerization reaction will begin; the temperature will start to rise, and the polymerization reactor temperature control program will activate the heat dissipation system, such as activating the jacketed cooling system to control the maximum temperature at 80-100℃.

[0103] 9) When the rate of temperature change is at its maximum (i.e., ΔT / Δt) max When the polymerization reactor temperature reaches 70–90°C, the second group of butadiene is added from the top feed inlets of the second and third polymerization reactors, respectively (the first group of butadiene was previously added from the bottom feed inlet). Once the polymerization reaction begins, the temperature inside the polymerization reactor will continue to rise, and the rate of temperature rise ΔT / Δt will become increasingly larger, until it begins to decrease at a certain point, which is ΔT / Δt. max ;

[0104] 10) When the second group of butadiene was added to the polymerization reactor, the highest temperature T was detected. max At that time, the back-end modifier was added. The polymerization reactor temperature control program detected T... max Afterwards, the chilled water in the cooling water jacket is stopped. The polymerization reactor temperature will continue to rise after the second batch of butadiene is added. Then, the rate of temperature rise will gradually decrease over time. The temperature at which the rate of temperature rise is ≤0.3℃ / min is T. max When the solvent / monomer value is set to 5-6, T max It's approximately 80-100℃. max After the cooling water in the jacket stops circulating, the jacket remains filled with chilled water, which can still carry away some of the reaction heat in the polymerization reactor.

[0105] 11) The coupling agent should be added 3-7 minutes after the downstream modifier is added;

[0106] 12) After the coupling agent is added, continue stirring for 10-20 minutes to complete the coupling process. The polymerization reaction is then complete, and the discharge procedure is initiated. After the reaction is complete, take a sample from the sampling point of the polymerization reactor to determine the Mooney viscosity (MV) and perform GPC analysis on the polymer solution sample.

[0107] After obtaining the MV and GPC analysis values ​​of the polymer solution sample from the polymerization reactor, check whether the analysis values ​​meet the process control standards. If both the MV and GPC analysis values ​​are within the allowable range of the process control standards, then after the reaction process is completed, discharge the polymer reactor into the flash evaporation system according to the following procedure:

[0108] a) The agitators in the second and third polymerization reactors stop operating;

[0109] b) Open the valves of the pressure balance lines between the second and third polymerization reactors and each feed tank;

[0110] c) The discharge valves of the second and third polymerization reactors are opened;

[0111] d) Open the glue receiving valve of the selected glue receiving tank;

[0112] e) Start the polymerization dispensing pump;

[0113] f) Add antioxidants;

[0114] g) When the liquid level in the second and third polymerization reactors drops to 1% (PL+1%) above the low liquid level warning (process low liquid level) setting value of the polymerization reactor level gauge, the dispensing pump stops operating;

[0115] h) The bottom discharge valves of the second and third polymerization reactors are closed;

[0116] i) The glue dispensing valve is closed;

[0117] j) Close the valves of the pressure balance line between the polymerization reactor and each feeding tank.

[0118] Table 1 shows the reference feed percentage, feed rate, and other parameters for the batch polymerization mode of solution-polymerized styrene-butadiene rubber.

[0119] Table 1

[0120]

[0121] Example 1

[0122] Initiating the continuous polymerization mode of solution-polymerized styrene-butadiene rubber:

[0123] (1) The first polymerization reactor 523, the second polymerization reactor 524 and the third polymerization reactor 525 are connected in series. The static mixer 527 is connected to the bottom feed port A1 of the first polymerization reactor 523 and the top discharge port A2 discharges into the bottom feed port B1 of the second polymerization reactor 524. The polymerization is further carried out in the second polymerization reactor 524. The discharge port B2 of the second polymerization reactor 524 discharges into the bottom feed port C1 of the third polymerization reactor 525. The polymerization is further carried out in the third polymerization reactor 525. Then the discharge port C2 of the third polymerization reactor 525 discharges into the flash evaporation system 6.

[0124] (2) The refined solvent from the solvent refining unit 3 and the flash evaporation system, after being preheated or precooled, is mixed with refined butadiene oil from the butadiene refining unit 1, refined benzene oil from the styrene refining unit 4, and refined isoprene from the isoprene refining unit 2. After adding scale inhibitor and activator, it enters the static mixer 526. Then, the catalyst is added and enters the static mixer 527. The feed temperature is controlled at 60±2℃. The feed amount of butadiene is set to 75 phm, the feed amount of styrene to 25 phm, the feed amount of refined solvent to 500 phm, the feed amount of catalyst to 0.025 phm, the molar ratio of activator to catalyst to 4.2, and the feed amount of scale inhibitor to 0.2 phm. Specifically, the temperature of the first polymerization reactor is controlled at 75±2℃ and the pressure is controlled at approximately 0.6 MPa, so that the monomer conversion rate reaches 99.5%; the temperature of the second polymerization reactor is controlled at 65±2℃ and the pressure is controlled at approximately 0.5 MPa; and the temperature of the third polymerization reactor is controlled at 65±2℃ and the pressure is controlled at approximately 0.5 MPa.

[0125] (3) After the adhesive solution enters the flash tank 61, flash evaporation occurs, and part of the solvent in the adhesive solution vaporizes and enters the flash solvent condenser 62 to condense into a liquid phase. Then, it enters the flash solvent condensate tank 63 and passes through the flash solvent molecular sieves (64, 65) to remove impurities from the solvent. The liquid is then returned to the feeding system. The flash-evaporated adhesive solution is sent to the coagulation unit, where the solvent in the coagulation kettles connected in series is removed. The removed solvent is refined and recycled. The coagulated rubber particles are sent to the post-processing unit for dehydration, drying, briquetting, and packaging before being shipped as rubber products.

[0126] The solution-polymerized styrene-butadiene rubber product Mooney 58-68 has a styrene content of 23-27%, a vinyl content of 62-64%, a glass transition temperature of -30℃±1℃, a number-average molecular weight (Mn) of 470-510 kg / mol PS, a weight-average molecular weight (Mw) of 910-950 kg / mol PS, a coupling efficiency of 45%-55%, and a filler oil content of 37.5±0.5 PHr.

[0127] Example 2

[0128] Based on Example 1, this embodiment stops the continuous polymerization mode and switches to the solution polymerization of styrene-butadiene rubber in a batch polymerization mode:

[0129] The first polymerization reactor 523 is temporarily suspended. The second polymerization reactor 524 and the third polymerization reactor 525 are connected in parallel. The second polymerization reactor 524 is connected to both the feeding system and the flash evaporation system 6. The third polymerization reactor 525 is connected to both the feeding system and the flash evaporation system 6.

[0130] (1) The refined solvent from the solvent refining unit 3 and the flash evaporation system, after passing through the preheater 528 and the precooler 529, is fed from the bottom feed port of the second and third polymerization reactors to maintain the temperature inside the second and third polymerization reactors at 20±2℃.

[0131] (2) When the amount of solvent added reaches 13t, start the agitator of the second and third polymerization reactors. The refined solvent of solvent refining unit 3 and flash evaporation system, after being combined with the first group of refined butadiene from butadiene refining unit 1, continues to be fed into the bottom feed port of the second and third polymerization reactors. At the same time as stirring is started, styrene, activator and front-end modifier are fed from the top feed port of the second and third polymerization reactors.

[0132] (3) Add the catalyst to the catalyst feeding tank according to the set amount; add the downstream modifier to the downstream modifier feeding tank according to the set amount;

[0133] (4) The feeding of the first group of butadiene, styrene, activator and front-end modifier is completed; among them, the feeding of butadiene, styrene, activator and front-end modifier is completed before the solvent feeding is completed;

[0134] (5) Check and confirm that the temperature inside the polymerization reactor is within the range of 20±2℃, add the catalyst into the polymerization reactor, and the polymerization reaction begins;

[0135] (6) As the polymerization reaction begins, the temperature inside the polymerization reactor rises. Turn on the rubber-sleeved chilled water and the internal cooling pipe assembly, as well as the reactor top condenser, to keep the temperature inside the polymerization reactor at 90±5℃.

[0136] (7) When the rate of temperature change is detected to be at its maximum (i.e., ΔT / Δt) max When the temperature of the polymerization reactor reaches approximately 85°C, the second group of butadiene is added from the top feed inlets of the second and third polymerization reactors, respectively.

[0137] (8) When the second group of butadiene was added to the polymerization reactor, the highest temperature T was detected. max When the polymerization reactor temperature rise rate is ≤0.3℃ / min, the downstream modifier is added. The polymerization reactor temperature control program detects T... max Then, stop the chilled water in the cooling water jacket.

[0138] (9) The coupling agent should be added 3-7 minutes after the downstream modifier is added;

[0139] (10) After the coupling agent is added, continue stirring for 10-20 minutes to complete the "coupling". The polymerization reaction process is over. After the inspection is qualified, start the discharge program.

[0140] (11) The polymerized solution is discharged from the bottom of the second polymerization reactor 524 and the third polymerization reactor 525 to the flash evaporation system 6. After entering the flash evaporation tank 61, the solution undergoes flash evaporation, during which part of the solvent in the solution vaporizes and enters the flash solvent condenser 62 to condense into a liquid phase. Then, it enters the flash solvent condensate tank 63 and passes through the flash solvent molecular sieves (64, 65) to remove impurities from the solvent. The solution is then returned to the feed system. The flash-evaporated solution is sent to the coagulation unit, where the solvent is removed from the solution in the coagulation tank. The removed solvent is then refined and recycled. The coagulated rubber particles are sent to the post-processing unit for dehydration, drying, briquetting, and packaging before being shipped as rubber products.

[0141] The application details of each component are shown in Table 2:

[0142] Table 2

[0143]

[0144] The solution-polymerized styrene-butadiene rubber product Mooney 69-79 produced by intermittent polymerization has a styrene content of 18-22%, a vinyl content of 53-57%, a glass transition temperature of -36℃±1℃, a number-average molecular weight (Mn) of 120-160 kg / mol PS, a weight-average molecular weight (Mw) of 160-200 kg / mol PS, and a coupling efficiency of 65%-75%.

[0145] Example 3

[0146] This embodiment, based on embodiment 2, stops the intermittent aggregation mode and switches to the continuous aggregation mode:

[0147] (1) The first polymerization reactor 523, the second polymerization reactor 524 and the third polymerization reactor 525 are connected in series. The static mixer 527 is connected to the bottom feed port A1 of the first polymerization reactor 523 and the top discharge port A2 discharges into the bottom feed port B1 of the second polymerization reactor 524. The polymerization is further carried out in the second polymerization reactor 524. The discharge port B2 of the second polymerization reactor 524 discharges into the bottom feed port C1 of the third polymerization reactor 525. The polymerization is further carried out in the third polymerization reactor 525. Then the discharge port C2 of the third polymerization reactor 525 discharges into the flash evaporation system 6.

[0148] (2) The refined solvent from the solvent refining unit 3 and the flash evaporation system, after being preheated or precooled, is mixed with refined butadiene oil from the butadiene refining unit 1, refined benzene oil from the styrene refining unit 4, and refined isoprene from the isoprene refining unit 2. After adding scale inhibitor and activator, it enters the static mixer 526. Then, the catalyst is added and it enters the static mixer 527. The feed temperature is controlled at 58±2℃. The feed amount of butadiene is set to 70 phm, the feed amount of styrene to 20 phm, the feed amount of refined solvent to 450 phm, the feed amount of catalyst to 0.02 phm, the molar ratio of activator to catalyst to 4.4, and the feed amount of scale inhibitor to 0.1 phm. Specifically, the temperature of the first polymerization reactor is controlled at 73±2℃ and the pressure is controlled at approximately 0.6 MPa, so that the monomer conversion rate reaches 99.2%; the temperature of the second polymerization reactor is controlled at 65±2℃ and the pressure is controlled at approximately 0.5 MPa; and the temperature of the third polymerization reactor is controlled at 65±2℃ and the pressure is controlled at approximately 0.5 MPa.

[0149] (3) After the adhesive solution enters the flash tank 61, flash evaporation occurs, and part of the solvent in the adhesive solution vaporizes and enters the flash solvent condenser 62 to condense into a liquid phase. Then, it enters the flash solvent condensate tank 63 and passes through the flash solvent molecular sieves (64, 65) to remove impurities from the solvent. The liquid is then returned to the feeding system. The flash-evaporated adhesive solution is sent to the coagulation unit, where the solvent in the coagulation kettles connected in series is removed. The removed solvent is refined and recycled. The coagulated rubber particles are sent to the post-processing unit for dehydration, drying, briquetting, and packaging before being shipped as rubber products.

[0150] The solution-polymerized styrene-butadiene rubber product Mooney 55-65 has a styrene content of 34-38%, a vinyl content of 38-42%, a glass transition temperature of -27℃±1℃, a number-average molecular weight (Mn) of 410-450 kg / mol PS, a weight-average molecular weight (Mw) of 800-840 kg / mol PS, a coupling efficiency of 45%-55%, and a filler oil content of 37.5±0.5 PHr.

[0151] The production equipment and process of this invention, through multiple improvements such as increasing the production capacity of the polymerization reactor, achieve the goal of flexibly switching between the production of two grades of solution-polymerized styrene-butadiene rubber on the same production line. The rubber products obtained from both continuous and intermittent production have good comprehensive performance and stability. Furthermore, the investment in modification based on existing equipment is relatively small, the energy consumption of the production process is low, and it can also be used to produce SB, LCBR, SIBR and other products as needed.

[0152] The preferred embodiments of the present invention have been described above to make the spirit of the present invention clearer and easier to understand, and are not intended to limit the present invention. All modifications, substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope summarized by the appended claims.

Claims

1. A flexible switching production equipment for solution-polymerized styrene-butadiene rubber, characterized in that, It includes a feeding system, a polymerization system, a flash evaporation system, and a condensation system connected in sequence; The polymerization system includes a first polymerization reactor, a second polymerization reactor, and a third polymerization reactor; The production equipment can flexibly switch between continuous polymerization mode and intermittent polymerization mode: The continuous polymerization mode includes: a first polymerization reactor, a second polymerization reactor, and a third polymerization reactor connected in series, with the first polymerization reactor connected to the feeding system and the third polymerization reactor connected to the flash evaporation system; The batch polymerization mode includes: a second polymerization reactor and a third polymerization reactor connected in parallel, the second polymerization reactor being connected to the feed system and the flash evaporation system respectively, and the third polymerization reactor being connected to the feed system and the flash evaporation system respectively; The feeding system includes a butadiene refining unit, an isoprene refining unit, a styrene refining unit, a solvent refining unit, a continuous polymerization aid unit for continuous polymerization mode, and a batch polymerization aid unit for batch polymerization mode. The continuous polymerization aid unit includes at least one of the following: a continuous polymerization catalyst feed port, a continuous polymerization activator feed port, a continuous polymerization scale inhibitor feed port, a continuous polymerization coupling agent feed port, and a continuous polymerization modifier feed port; The batch polymerization aid unit includes at least one of the following: batch polymerization catalyst feed port, batch polymerization activator feed port, batch polymerization front-end modifier feed port, batch polymerization back-end modifier feed port, and batch polymerization coupling agent feed port; In continuous polymerization mode, the feeding system is connected to the bottom inlet A1 of the first polymerization reactor after passing through the mixer. The top outlet A2 of the first polymerization reactor is connected to the bottom inlet B1 of the second polymerization reactor. The top outlet B2 of the second polymerization reactor is connected to the bottom inlet C1 of the third polymerization reactor. The top outlet C2 of the third polymerization reactor is connected to the flash evaporation system. In the batch polymerization mode, the solvent purification unit is connected to the bottom feed port B1 of the second polymerization reactor and the bottom feed port C1 of the third polymerization reactor, respectively. The isoprene refining unit and the styrene refining unit are respectively connected to the top feed port B3 of the second polymerization reactor and the top feed port C3 of the third polymerization reactor; The butadiene refining unit is connected to the bottom feed port B1 and top feed port B3 of the second polymerization reactor, and to the bottom feed port C1 and top feed port C3 of the third polymerization reactor. Each feed port in the batch polymerization aid unit is connected to the top feed port B3 of the second polymerization reactor and the top feed port C3 of the third polymerization reactor, respectively.

2. The production equipment as described in claim 1, characterized in that, In the batch polymerization mode, the bottom outlet B4 of the second polymerization reactor and the bottom outlet C4 of the third polymerization reactor are connected to the flash evaporation system, respectively.

3. The production equipment as described in claim 1 or 2, characterized in that, The volumes of the second and third polymerization reactors are 1.5-2.5 times the volume of the first polymerization reactor, respectively. The second and third polymerization reactors are each equipped with a heat dissipation system, which includes a jacketed cooler and several internal cooling pipe groups. The jacketed cooler includes a cooling water jacket covering the outer wall of the polymerization reactor, a cooling water inlet at the bottom of the cooling water jacket, and several cooling water outlets at the top of the cooling water jacket. The internal cooling tube assembly includes multiple internal cooling vertical tubes extending axially along the polymerization reactor, and the surface roughness Ra of the internal cooling vertical tubes is ≤0.1μm.

4. The production equipment as described in claim 3, characterized in that, The volumes of the second and third polymerization reactors are greater than 70 m³. 3 .

5. The production equipment as described in claim 3, characterized in that, The heat dissipation system also includes heat dissipation agitators arranged axially along the interior of the second and third polymerization reactors. Each heat dissipation agitator includes a rotating shaft and a wide-width stirring paddle connected to the rotating shaft. The rotating shaft and the wide-width stirring paddle have a cooling water passage. The width of the wide-width stirring paddle accounts for 60-90% of the internal diameter of the polymerization reactor, and its height accounts for 60-90% of the internal height of the polymerization reactor.

6. The production equipment as described in claim 5, characterized in that, The flash evaporation system includes a flash tank, a solvent condenser, a flash solution condensate tank, and a flash solvent molecular sieve. The liquid phase outlet of the flash tank is connected to the condensation unit, and the gas phase outlet is connected in sequence to the solvent condenser, the flash solution condensate tank, and the flash solvent molecular sieve, so that the cooled and refined solvent is returned to the feeding system.

7. A flexible switching production method for solution-polymerized styrene-butadiene rubber (SBR), wherein the production method utilizes the flexible switching production equipment for SBR according to any one of claims 1-6, characterized in that, The production method flexibly switches between continuous polymerization and batch polymerization modes by changing the connection method of the feeding system, polymerization system, and flash evaporation system; including: (1) Connect the first polymerization reactor, the second polymerization reactor and the third polymerization reactor in series. The first polymerization reactor is connected to the feeding system and the third polymerization reactor is connected to the flash evaporation system to enter the continuous polymerization mode; (2) Connect the second polymerization reactor and the third polymerization reactor in parallel. The second polymerization reactor is connected to the feeding system and the flash evaporation system respectively, and the third polymerization reactor is connected to the feeding system and the flash evaporation system respectively, and enter the batch polymerization mode.

8. The production method as described in claim 7, characterized in that, In intermittent aggregation mode, The refined solvent is fed through the bottom inlet B1 of the second polymerization reactor and the bottom inlet C1 of the third polymerization reactor, respectively. Refined isoprene and refined styrene are fed through the top inlet B3 of the second polymerization reactor and the top inlet C3 of the third polymerization reactor, respectively. Refined butadiene is fed into the second polymerization reactor through the bottom feed port B1 and the top feed port B3, respectively, and into the third polymerization reactor through the bottom feed port C1 and the top feed port C3, respectively. The batch polymerization aid is fed through the top feed port B3 of the second polymerization reactor and the top feed port C3 of the third polymerization reactor, respectively.

Citation Information

Patent Citations

  • External circulation reactor, and heat removal method for polymerization reaction

    CN113941296A

  • Chemical reactor integrated configuration of multipurpose

    CN208389990U