Modified y molecular sieve, preparation method and application thereof, and method for removing nitrogen-containing basic substances in benzene
By synthesizing and modifying Y molecular sieves using a microwave method, the problem of balancing strength and crystallinity of binder-free Y molecular sieves under high temperature and high alkalinity conditions was solved, achieving efficient adsorption of nitrogen-containing alkaline substances in benzene and improving adsorption performance and service life.
Patent Information
- Application Number
- CN202211320487.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-26
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-10-26
AI Technical Summary
Existing Y molecular sieves have shortcomings in adsorption performance, especially in removing nitrogen-containing alkaline substances from benzene. Furthermore, when synthesizing binder-free molecular sieves under high temperature and high alkaline conditions, it is difficult to achieve both strength and crystallinity.
A binder-free Y molecular sieve was synthesized using a microwave method, and its adsorption performance was improved by introducing ZnO, lanthanide metal oxides, and iron-based metal oxides through an exchange method.
The prepared modified Y molecular sieve exhibits both high strength and high crystallinity under low temperature and low alkali conditions, which significantly improves the adsorption performance of nitrogen-containing alkaline substances in benzene and extends the service life of the adsorbent.
Smart Images

Figure CN117920133B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of molecular sieve technology, specifically to a modified Y molecular sieve, its preparation method, application, and method for removing nitrogen-containing alkaline substances from benzene. Background Technology
[0002] Ethylbenzene is an important petrochemical raw material, mainly used in the production of styrene, which is the primary raw material for the production of polystyrene and other polyresins. The main production methods for ethylbenzene involve the alkylation of benzene and ethylene, divided into molecular sieve gas-phase and molecular sieve liquid-phase methods. The molecular sieve liquid-phase method has slight advantages in terms of material and energy consumption, making it the most mainstream production method. In the early 1990s, Lummus and UOP introduced a molecular sieve liquid-phase alkylation process for ethylbenzene. This process uses β and Y-type zeolite molecular sieves as catalysts and has advantages such as low reaction temperature, ease of operation, and fewer byproducts. Patent applications US4891458, US5227558, and CN1506340A describe this process in detail. In the mid-1990s, liquid-phase alkylation and gas-phase alkylation processes for ethylbenzene were introduced. This process uses MCM-22 as a molecular sieve liquid-phase alkylation catalyst and has advantages such as a low benzene-to-ethylene ratio and fewer byproducts. Patent application CN1171096A describes this process in detail.
[0003] The liquid-phase alkylation of benzene and ethylene to produce ethylbenzene typically occurs at temperatures between 180-250℃. The catalyst exhibits poor resistance to poisoning; even trace amounts of nitrogenous alkaline substances in benzene can poison the catalyst. To ensure stable catalyst operation, it is necessary to remove nitrogenous alkaline substances from the benzene, reducing the nitrogen content to below 0.1 mg / L. Current production processes commonly use bleaching clay and molecular sieves (e.g., 13X) to pretreat benzene and reduce its alkaline nitrogen content. However, the adsorbent has a short service life, requiring replacement or regeneration every three to six months, or even less, before losing its performance and poisoning the catalyst. Therefore, adsorbents with greater nitrogen adsorption capacity are needed to extend their replacement cycle.
[0004] Molecular sieves with relatively low silica-to-alumina ratios, such as type A, X, or Y molecular sieves, are often used as adsorbents. Metal modification can often improve their adsorption performance. However, to meet industrial requirements, especially size and strength requirements, molecular sieves, binders, and additives need to be mixed and molded to produce adsorbents with specific size and strength. However, the addition of binders and additives can cover the active sites of the molecular sieve and limit the molecular sieve content in the adsorbent. To increase the molecular sieve content and enhance the adsorption performance of denitrifying agents, synthesizing binder-free molecular sieves is an effective approach. Patent application CN107511162A reports a method for synthesizing binder-free Y molecular sieves. However, this technique uses 40-90% of the synthesized Y molecular sieve and silicon-containing compounds, resulting in secondary crystallization and a complex synthesis process. Furthermore, the binder converted from the silicon-containing compounds does not contain aluminum and fails to effectively improve adsorption performance. Transition metal oxides are often used to modify molecular sieves to improve their adsorption performance; for example, patent application CN101591213A uses Cs... + Mg 2+ Ce 3+ La 3+ Zn 2+ and Mn 2+ Modified Y molecular sieves are used to remove acidic substances such as thiols and sulfur dioxide, but not for adsorbing nitrogen-containing alkaline substances.
[0005] In microwave heating reaction, microwaves are continuously absorbed as they pass through the reactants, resulting in deep heating, or "internal heating." At the same time, the products also act as autocatalysts while absorbing microwaves. Therefore, microwaves are often used in the synthesis of molecular sieves. We used the microwave method to synthesize binder-free high-silica ZSM-5 molecular sieve. Summary of the Invention
[0006] The purpose of this invention is to overcome the problem that the adsorption performance of Y-type molecular sieves in the prior art needs further improvement, and to provide a modified Y-type molecular sieve, its preparation method, application, and method for removing nitrogen-containing basic substances from benzene. This modified Y-type molecular sieve exhibits excellent adsorption performance.
[0007] To achieve the above objectives, the present invention provides a modified Y molecular sieve, which contains Y molecular sieve, ZnO, lanthanide metal oxides, iron metal oxides, and optionally a binder.
[0008] Based on the total weight of the modified Y molecular sieve, the content of Y molecular sieve is 60-80% by weight, the content of ZnO is 10-25% by weight, the content of lanthanide metal oxides is 2-10% by weight, the content of iron metal oxides is 2-10% by weight, and the content of binder is less than 2% by weight.
[0009] Y-type molecular sieves differ from the synthesis of high-silica ZSM-5. The synthesis of high-silica ZSM-5 often requires organic amines as template agents and has low basicity requirements; for example, the basicity of organic amines such as ethylamine and n-methylamine is sufficient for synthesis. In contrast, the synthesis of Y-type molecular sieves generally uses an amine-free method, but requires crystallization under higher temperature and basicity conditions. Binder-free molecular sieves are mainly composed of silicon-aluminum oxides, which are prone to partial dissolution under higher temperature and basicity conditions, affecting their strength. Furthermore, coarser strands are beneficial for improving the strength of Y-type molecular sieves, but in traditional binder-free synthesis methods, larger particles are detrimental to crystallization.
[0010] A second aspect of this invention provides a method for preparing modified Y molecular sieves, the method comprising the following steps:
[0011] 1) Y seed crystals, aluminum source, silicon source, adhesive solvent and optional pore-forming agent are kneaded together to obtain binder-free Y molecular sieve precursor;
[0012] 2) The binderless Y molecular sieve precursor is liquid-phase crystallized under microwave conditions, and the relative crystallinity of the binderless Y molecular sieve in the crystallization product is above 98%.
[0013] 3) Exchange the binder-free Y molecular sieve obtained in step 2) with an aqueous solution containing zinc compound;
[0014] 4) Load the solid product obtained in step 3) with lanthanide and iron-based metal compounds to obtain modified Y molecular sieve.
[0015] In existing technologies, the synthesis of Y-type molecular sieves generally uses an amine-free method, but this requires crystallization under high temperature and alkalinity conditions. During the research process, the researchers of this invention discovered that binder-free Y-type molecular sieves are prone to partial dissolution under high temperature and alkalinity conditions, affecting their strength. Although the strength of binder-free Y-type molecular sieves can be improved by molding them into coarser strips, larger particles are not conducive to crystallization, resulting in a defect where it is difficult to simultaneously achieve high strength and relative crystallinity in the prepared binder-free Y-type molecular sieves, severely reducing their adsorption performance. The researchers of this invention further discovered that, under certain conditions, binder-free Y-type molecular sieves with both high strength and relative crystallinity can be obtained, improving their adsorption performance. Furthermore, modification can further enhance their excellent adsorption properties. This invention first synthesizes binder-free Y-type molecular sieves with both high strength and relative crystallinity using a microwave method at low temperature and low alkalinity. Then, through exchange, zinc-containing compounds are introduced into the pores of the binder-free Y-type molecular sieve, which is beneficial for improving its adsorption performance. Finally, further modification with lanthanide and iron-based metal compounds further improves its adsorption performance.
[0016] The third aspect of this invention provides the application of the modified Y molecular sieve described in the first aspect or the modified Y molecular sieve prepared by the method described in the second aspect in denitrification.
[0017] A fourth aspect of the present invention provides a method for removing nitrogen-containing basic substances from benzene, the method comprising: contacting the benzene containing nitrogen-containing basic substances with a denitrifying agent, wherein the denitrifying agent comprises the modified Y molecular sieve described in the first aspect or the modified Y molecular sieve prepared by the method described in the second aspect.
[0018] The beneficial effects of the present invention through the above technical solution include:
[0019] The modified Y molecular sieve provided by this invention utilizes the synergistic effect of Y molecular sieve, ZnO, lanthanide metal oxides and iron metal oxides. Moreover, the binder content in the modified Y molecular sieve is extremely low, which has virtually no impact on the performance of the modified Y molecular sieve, resulting in excellent adsorption performance. Attached Figure Description
[0020] Figure 1 This is the XRD pattern of the binder-free Y molecular sieve prepared in Example 1.
[0021] Figure 2 It is the breakthrough curve of nitrogen-containing alkaline substances adsorbed by the denitrifying agent containing the modified Y molecular sieve prepared in Example 1. Detailed Implementation
[0022] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0023] In one aspect, the present invention provides a modified Y molecular sieve, which contains Y molecular sieve, ZnO, lanthanide metal oxides, iron metal oxides, and optionally a binder;
[0024] Based on the total weight of the modified Y molecular sieve, the content of Y molecular sieve is 60-80% by weight, the content of ZnO is 10-25% by weight, the content of lanthanide metal oxides is 2-10% by weight, the content of iron metal oxides is 2-10% by weight, and the content of binder is less than 2% by weight.
[0025] In this invention, the binder content in the modified Y molecular sieve is less than 2% by weight, which has virtually no impact on the performance of the modified Y molecular sieve, and the modified Y molecular sieve contains virtually no binder.
[0026] The binder described in this invention is SiO2 that has not formed a Y molecular sieve.
[0027] According to the present invention, preferably, based on the total weight of the modified Y molecular sieve, the content of Y molecular sieve is 65-75% by weight, the content of ZnO is 15-22% by weight, the content of lanthanide metal oxides is 2-8% by weight, and the content of iron metal oxides is 2-8% by weight.
[0028] The total content of each component in the modified Y molecular sieve of this invention is 100%.
[0029] The content of each component in the modified Y molecular sieve of the present invention was determined by XRF method, and the binder was calculated according to crystallinity.
[0030] According to the present invention, preferably, the weight ratio of ZnO, lanthanide metal oxide, and iron-based metal oxide is 1:0.05-0.5:0.05-0.4, more preferably 1:0.1-0.35:0.1-0.3. This preferred embodiment is beneficial for improving the adsorption performance of the modified Y molecular sieve.
[0031] According to the present invention, preferably, the Na2O content in the modified Y molecular sieve is less than 2% by weight, and more preferably 0.5-1.5% by weight.
[0032] The Na2O content in the modified Y molecular sieve of the present invention was determined by XRF method.
[0033] According to the present invention, preferably, the modified Y molecular sieve has a cross-sectional diameter of 3.5-7 mm, more preferably 4-6.5 mm; and a length of 5-50 mm, more preferably 7-25 mm. This preferred embodiment can further improve the strength of the modified Y molecular sieve.
[0034] The dimensions of the modified Y molecular sieve described in this invention were measured using vernier calipers.
[0035] In existing binder-free Y molecular sieves, the strength is generally between 60-120 N / cm. The modified Y molecular sieve of the present invention has higher strength. Preferably, the lateral compressive strength of the modified Y molecular sieve is 125-170 N / cm, and more preferably 125-150 N / cm.
[0036] The lateral compressive strength of the modified Y molecular sieve described in this invention is tested using a pressure testing machine. The testing method is as follows: the modified molecular sieve is cut into particles with a length L of 0.4-0.6 cm, the particles are placed laterally on the testing platform, and the pressure is gradually increased until the particles are crushed. The instrument records the pressure F applied when the particles are crushed. F / L is the compressive strength of a single modified Y molecular sieve particle. The lateral compressive strength of the modified Y molecular sieve is obtained by averaging the compressive strength of 20 particles.
[0037] According to the present invention, preferably, the SiO2 / Al2O3 molar ratio of the modified Y molecular sieve is 5-20, more preferably 5-10.
[0038] The SiO2 / Al2O3 molar ratio of the modified Y molecular sieve described in this invention was determined by XRF method.
[0039] The present invention allows for a wide range of lanthanide metals, and various lanthanide metals commonly used in the art can be used. Preferably, the lanthanide metal is selected from at least one of La, Ce, Pr, and Pm, and more preferably La and / or Ce.
[0040] According to the present invention, preferably, the iron-based metal is selected from at least one of Ni, Co and Fe, and more preferably Ni and / or Co.
[0041] According to a preferred embodiment of the present invention, the modified Y molecular sieve comprises Y molecular sieve, ZnO, lanthanide metal oxides, iron-based metal oxides, and a binder; the lanthanide metal is La and / or Ce, and the iron-based metal is Ni and / or Co; based on the total weight of the modified Y molecular sieve, the content of Y molecular sieve is 65-75% by weight, the content of ZnO is 15-22% by weight, the content of lanthanide metal oxides is 2-8% by weight, and the content of iron-based metal oxides is 2-8% by weight; the content of the binder is less than 2% by weight. The modified Y molecular sieve of the present invention exhibits excellent adsorption performance.
[0042] A second aspect of this invention provides a method for preparing modified Y molecular sieves, the method comprising the following steps:
[0043] 1) Y seed crystals, aluminum source, silicon source, adhesive solvent and optional pore-forming agent are kneaded together to obtain binder-free Y molecular sieve precursor;
[0044] 2) The binderless Y molecular sieve precursor is liquid-phase crystallized under microwave conditions, and the relative crystallinity of the binderless Y molecular sieve in the crystallization product is above 98%.
[0045] 3) Exchange the binder-free Y molecular sieve obtained in step 2) with an aqueous solution containing zinc compound;
[0046] 4) Load the solid product obtained in step 3) with lanthanide and iron-based metal compounds to obtain modified Y molecular sieve.
[0047] According to the present invention, preferably, the amounts of zinc compound, lanthanide metal compound and iron metal compound are such that, based on the total weight of the modified Y molecular sieve, the content of Y molecular sieve is 60-80% by weight, the content of ZnO is 10-25% by weight, the content of lanthanide metal oxide is 2-10% by weight, and the content of iron metal oxide is 2-10% by weight.
[0048] According to the present invention, preferably, the amounts of zinc compound, lanthanide metal compound and iron metal compound are such that, based on the total weight of the modified Y molecular sieve, the content of Y molecular sieve is 65-75% by weight, the content of ZnO is 15-22% by weight, the content of lanthanide metal oxide is 2-8% by weight, and the content of iron metal oxide is 2-8% by weight.
[0049] According to the present invention, preferably, the amounts of zinc compound, lanthanide metal compound and iron metal compound are such that the weight ratio of ZnO, lanthanide metal oxide and iron metal oxide in the prepared modified Y molecular sieve is 1:0.05-0.5:0.05-0.4, more preferably 1:0.1-0.35:0.1-0.3.
[0050] The present invention allows for a wide range of choices of the adhesive solvent, including various adhesive solvents conventionally used in the art. According to the present invention, preferably, the adhesive solvent is an inorganic acid, more preferably nitric acid.
[0051] Preferably, the adhesive solvent of the present invention is provided in the form of an aqueous solution. Preferably, the concentration of the aqueous solution of the adhesive solvent is 1-10 wt%.
[0052] The present invention does not impose a particular limitation on the amount of the aqueous solution of the adhesive solvent, which can be appropriately selected according to specific circumstances. Preferably, the amount of the aqueous solution of the adhesive solvent is 8-40% of the total weight of the Y seed crystal, aluminum source, and silicon source in step 1).
[0053] In this invention, unless otherwise specified, "optional" means containing or not containing, adding or not adding, or using or not using. Specifically, step (c) of this invention may or may not involve the addition of a pore-forming agent.
[0054] The present invention has a wide range of choices for the pore-forming agent. Preferably, the pore-forming agent is fennel powder and / or methylcellulose.
[0055] The present invention does not impose a particular limitation on the amount of the pore-forming agent, which can be appropriately selected according to specific circumstances. Preferably, the amount of the pore-forming agent is 0.2-2.5% of the total weight of the Y-seed, aluminum source, and silicon source in step 1).
[0056] The present invention does not impose any particular limitation on the molding process in step (1), and it can be carried out according to conventional molding methods in the art. Preferably, the molding process in step (1) is extrusion molding. Specific methods are well known to those skilled in the art and will not be described in detail here.
[0057] This invention does not impose any particular limitation on the method of adding the Y-seed crystal, aluminum source, silicon source, adhesive solvent, and pore-forming agent; they can be added separately or together. This invention uses the method of adding them together as an example.
[0058] In existing technologies, the synthesis of Y-type molecular sieves generally uses an amine-free method, but this requires crystallization under high temperature and alkalinity conditions. However, binder-free molecular sieves are prone to partial dissolution under these conditions, affecting their strength. While thicker strips can improve the strength of binder-free Y-type molecular sieves, larger particles are detrimental to crystallization. To avoid affecting the crystallization effect, the diameter of the binder-free Y-type molecular sieve precursor in existing technologies is generally 1-2 mm. The method of this invention overcomes this defect, producing a binder-free Y-type molecular sieve with both high relative crystallinity and significantly higher strength. To improve the strength of the binder-free Y-type molecular sieve, preferably, the cross-sectional diameter of the binder-free Y-type molecular sieve precursor is 3.5-7 mm, more preferably 4-6.5 mm; and the length is 5-50 mm, more preferably 7-25 mm. Since the dimensions have virtually no impact on subsequent operations, the dimensions of the binder-free Y-type molecular sieve precursor are essentially the same as those of the modified Y-type molecular sieve.
[0059] According to the present invention, preferably, the weight content of SiO2 in the Y seed crystal is 1-15%, more preferably 5-10%, based on the total SiO2 weight in the binderless Y molecular sieve precursor.
[0060] According to the present invention, preferably, the molar ratio of silicon source to aluminum source is 5-20:1, more preferably 5-10:1, wherein the silicon source is SiO2 and the aluminum source is Al2O3.
[0061] The Y-seed crystals used in this invention can be commercially available or prepared using conventional methods. Preferably, they are prepared using a hydrothermal crystallization method, specifically by hydrothermal crystallization of a mixture of silicon compound, aluminum compound, alkali, and water.
[0062] Preferably, the molar ratio of the silicon compound, aluminum compound, alkali source and water is 1:(0.05-0.2):(0.3-0.7):(10-60), wherein the silicon compound is calculated as SiO2 and the aluminum compound is calculated as Al2O3.
[0063] Preferably, the crystallization conditions include: a temperature of 60-100℃ and a time of 10-30h.
[0064] Preferably, the crystallization is carried out under stirring conditions. The stirring rate and time can be appropriately selected according to specific circumstances.
[0065] Preferably, the selection of the silicon compound, aluminum compound, and alkali source is a conventional choice in the art, and will not be elaborated further here.
[0066] The present invention allows for a wide range of choices for the aluminum source, as long as aluminum can be provided. Preferably, the aluminum source is a soluble salt of aluminum, and is preferably selected from at least one of aluminum sulfate, aluminum nitrate, and aluminum acetate.
[0067] The present invention allows for a wide range of silicon sources, which can be various silicon sources conventionally used in the art. Specifically, the silicon source is an organosilicon source and / or an inorganic silicon source. Preferably, the silicon source is selected from at least one of silicon powder, silica, and silica sol.
[0068] Preferably, the method further includes: drying the molded article obtained in step 1) to obtain a binder-free Y molecular sieve precursor. The drying conditions can be carried out under conventional conditions, which will not be described in detail here.
[0069] According to the present invention, preferably, the relative crystallinity of the binder-free Y molecular sieve in the crystallized product is 98-100%.
[0070] The relative crystallinity mentioned in this invention refers to the ratio of the peak area of the eight crystal plane diffraction peaks (331), (511), (440), (533), (642), (660), (555), and (664) in the XRD characterization results of the sample to the peak area of the corresponding eight crystal plane diffraction peaks of the reference material.
[0071] According to the present invention, preferably, the liquid-phase crystallization under microwave conditions in step 2) includes: mixing the binderless Y molecular sieve precursor and an alkaline solution and then crystallizing under microwave conditions. This preferred embodiment is beneficial for improving the relative crystallinity of the binderless Y molecular sieve in the crystallized product.
[0072] Preferably, the weight ratio of the alkaline solution to the binder-free Y molecular sieve precursor is (0.8-3):1, more preferably 1.1-2:1.
[0073] This invention utilizes crystallization under low-alkali conditions, effectively avoiding the problem of partial dissolution of the binderless Y molecular sieve, which affects its strength. Preferably, the concentration of the alkaline solution is 1-5 wt%.
[0074] The present invention allows for a wide range of alkaline sources, including various alkaline sources commonly used in the art. Preferably, the alkaline source is selected from at least one of NaOH, KOH, and CsOH.
[0075] According to the present invention, preferably, the crystallization conditions include: a temperature of 40-100℃, more preferably 60-95℃; a time of 0.15-12 hours, more preferably 1-8 hours; and a microwave power of 100-900W, more preferably 300-700W. This preferred embodiment further improves the relative crystallinity of the binder-free Y molecular sieve in the crystallization product.
[0076] Preferably, the method further includes: performing solid-liquid separation and washing on the crystallized product obtained in step 2) to obtain binder-free Y molecular sieve.
[0077] The present invention does not impose any particular limitation on the solid-liquid separation and washing, which can be carried out in accordance with conventional technical means in the field, and will not be described in detail here.
[0078] According to the present invention, preferably, the conditions for the exchange include: a temperature of 30-70°C, more preferably 35-60°C; and a time of 1-10 hours, more preferably 2-5 hours.
[0079] In this invention, the exchange in step 3) can be performed once or multiple times. There is no particular limitation on this, as long as the ZnO content in the modified Y molecular sieve is within the aforementioned range. Preferably, the number of exchanges is 1-5 times, more preferably 2-4 times.
[0080] According to the present invention, preferably, the weight ratio of the binder-free Y molecular sieve to the aqueous solution of the zinc compound is 3-20:1, more preferably 5-10:1.
[0081] According to the present invention, preferably, the concentration of the aqueous solution of the zinc-containing compound is 0.5-2 mol / L.
[0082] According to the present invention, preferably, the zinc-containing compound is a soluble salt of zinc, preferably Zn(NO3)2 and / or ZnCl2.
[0083] According to a preferred embodiment of the present invention, the product of zinc exchange is first dried to obtain the solid product. The drying conditions can be carried out under conventional conditions, which will not be described in detail here.
[0084] This invention does not impose any particular limitation on the order in which lanthanide and iron-based metal compounds are loaded; they can be loaded together or separately. The preferred method is co-loading.
[0085] In this invention, there are no specific limitations on the method for loading lanthanide and iron-based metal compounds; conventional techniques in the art can be used for preparation. The impregnation method is preferred in this invention. The impregnation method includes: impregnating the solid product obtained in step 3) with an impregnation solution containing lanthanide and iron-based metal compounds, followed by optional drying. The drying conditions can be performed under conventional conditions, which will not be elaborated further here.
[0086] Preferably, the total weight ratio of lanthanide and iron-based metal compounds (calculated as oxides) to the zinc-modified Y molecular sieve is 10-12:1.
[0087] Preferably, in the impregnation solution containing lanthanide and iron-based metal compounds, the concentration of lanthanide metal compounds is 1.6-15 wt%, and the concentration of iron-based metal compounds is 1.5-12 wt%.
[0088] The present invention allows for a wide range of lanthanide metals, and various lanthanide metals commonly used in the art can be used. Preferably, the lanthanide metal is selected from at least one of La, Ce, Pr, and Pm, and more preferably La and / or Ce.
[0089] According to the present invention, preferably, the lanthanide metal compound is a soluble salt of a lanthanide metal, and is preferably selected from at least one of cerium nitrate, cerium chloride, lanthanum nitrate and lanthanum chloride.
[0090] According to the present invention, preferably, the iron-based metal is selected from at least one of Ni, Co and Fe, and more preferably Ni and / or Co.
[0091] According to the present invention, preferably, the iron-based metal compound is a soluble salt of an iron-based metal, and is preferably selected from at least one of cobalt nitrate, cobalt chloride, nickel nitrate, and nickel chloride.
[0092] According to the present invention, preferably, the method further includes: calcining the loaded lanthanide metal compound and iron metal compound in step 4).
[0093] The present invention does not impose any particular limitation on the roasting process, and can refer to methods commonly used in the art. Preferably, the roasting conditions include: a temperature of 450-600℃, more preferably 500-550℃; and a time of 2-12 hours, more preferably 4-8 hours. The roasting is generally carried out in an air atmosphere, which may include a flowing atmosphere or a stationary atmosphere.
[0094] The third aspect of the present invention provides the application of the modified Y molecular sieve described in the first aspect or the modified Y molecular sieve prepared by the method described in the second aspect in denitrification, preferably in the removal of nitrogen-containing alkaline substances from benzene.
[0095] A fourth aspect of the present invention provides a method for removing nitrogen-containing basic substances from benzene, the method comprising: contacting the benzene containing nitrogen-containing basic substances with a denitrifying agent, wherein the denitrifying agent comprises the modified Y molecular sieve described in the first aspect or the modified Y molecular sieve prepared by the method described in the second aspect.
[0096] The denitrifying agent of the present invention has strong adsorption performance. Preferably, in the material obtained by contact, the nitrogen-containing alkaline substances are reduced to below 0.1 mg / L based on the total nitrogen content.
[0097] The nitrogen content of the nitrogen-containing alkaline substance described in this invention is determined by a sulfur-nitrogen analyzer.
[0098] Preferably, the nitrogen penetration adsorption capacity of the denitrifying agent is above 10 mg / g, and more preferably 12-15 mg / g.
[0099] The nitrogen adsorption capacity of the denitrifying agent described in this invention is determined by breakthrough curve. Specifically, benzene containing nitrogenous alkaline substances flows through contact with the denitrifying agent, and samples are taken at regular intervals to measure the nitrogen content in the benzene. When the nitrogenous alkaline substances are above 0.1 mg / L, that is, when breakthrough occurs, the adsorption capacity is calculated based on the breakthrough time and concentration.
[0100] According to the present invention, preferably, the contact conditions include: a temperature of 40-200°C, more preferably 60-160°C; a pressure of 0.1-2 MPa, more preferably 0.5-1 MPa; and a mass hourly space velocity of 10-60 mL / g / h, more preferably 20-45 mL / g / h.
[0101] According to the present invention, preferably, the content of the nitrogen-containing alkaline substance is 1-50 mg / L, more preferably 5-15 mg / L.
[0102] According to the present invention, preferably, the nitrogen-containing basic substance comprises at least one of pyridine, quinoline and aniline.
[0103] The present invention will be described in detail below through embodiments.
[0104] In the following examples, the methods for determining the content of each component and the lateral pressure strength in the modified Y molecular sieve are as described above;
[0105] The XRD pattern of binderless Y molecular sieve was obtained by X-ray diffraction.
[0106] The raw materials used in the following examples are all commercially available products.
[0107] Example 1
[0108] a) Synthesis of Y molecular sieve seed crystals: Alkaline silica sol, aluminum sulfate octadecylhydrate, sodium hydroxide and water were used as raw materials. The material ratio (molar ratio) was: SiO2 / Al2O3 = 6, NaOH / SiO2 = 0.6, H2O / SiO2 = 20. The mixture was crystallized in a stainless steel reactor at 90°C for 20 hours under stirring to obtain a slurry material for later use. The SiO2 content was about 14 wt%.
[0109] b) Preparation of binder-free Y molecular sieve precursor: 21.3g of the above-mentioned Y molecular sieve seed crystals, 21.3g of silicon powder, 61.6g of alkaline silica sol (SiO2 content of 40wt%), 84.3g of aluminum sulfate octadecylhydrate, 0.5g of methylcellulose and 18.2g of nitric acid aqueous solution with a concentration of 7wt% were mixed evenly. The SiO2 / Al2O3 ratio in the mixture was 6. The mixture was extruded to obtain cylindrical strips with a diameter of 4.5mm, and then cut into particles with a length of 8-12mm. The particles were dried at 150℃ for 8h.
[0110] c) 10 g of the Y molecular sieve precursor obtained above was placed in 12 g of a 4 wt% NaOH aqueous solution, placed in a microwave reactor, heated to 90 °C, and crystallized at a microwave power of 300 W for 2 h. Then, solid-liquid separation and washing were performed to obtain a non-binding Y molecular sieve with a relative crystallinity of 98.5%. Figure 1 Its XRD pattern.
[0111] d) The unbonded Y molecular sieve was exchanged twice with a 0.5 mol / L zinc nitrate aqueous solution at a temperature of 55 °C for 3 h. The weight ratio of zinc nitrate aqueous solution to unbonded Y molecular sieve was 7:1. After drying at 120 °C for 12 h, a solid product was obtained.
[0112] e) Take 10g of the solid product and immerse it in an aqueous solution of 15g Ce(NO3)3 and Co(NO3)2, where the mass concentrations of Ce(NO3)3 and Co(NO3)2 are 5% and 3%, respectively. Dry the mixture at 150℃ for 8 hours, then calcine it at 500℃ for 4 hours to obtain the modified Y molecular sieve, whose size is basically the same as that of the Y molecular sieve precursor. The specific composition is shown in Table 1. Its lateral compressive strength was measured to be 135 N / cm.
[0113] An exemplary XRD pattern of the prepared binder-free Y molecular sieve is given. It can be seen that the diffraction peaks near 2θ = 6.18°, 10.13°, 11.89°, 15.66°, 18.70°, 20.35°, 23.65°, 27.06°, 31.41° and 34.09° are consistent with the characteristic diffraction peaks of Y molecular sieve, indicating that Y molecular sieve was successfully prepared.
[0114] Example 2
[0115] a) Preparation of binderless Y molecular sieve precursor: 33.2g of the slurry material obtained in step a of Example 1, 30.5g of silicon powder, 63.3g of alkaline silica sol (SiO2 content of 40wt%), 68.1g of aluminum sulfate octadecylhydrate, 0.6g of methylcellulose and 21.5g of nitric acid aqueous solution with a concentration of 6wt% were mixed evenly. The SiO2 / Al2O3 ratio in the mixture was 7.7. The mixture was extruded to obtain cylindrical strips with a diameter of 5.5mm, and then cut into particles with a length of 10-14mm. The particles were dried at 150℃ for 12h.
[0116] b) Place 10g of the Y molecular sieve precursor obtained above in 19g of KOH aqueous solution with a concentration of 4wt%, place it in a microwave reactor, heat it to 65℃, and crystallize it for 8h at a microwave power of 700W. Then, perform solid-liquid separation and washing to obtain a non-bonded Y molecular sieve with a relative crystallinity of 98.8%.
[0117] c) The unbonded Y molecular sieve was exchanged three times with a 0.6 mol / L zinc nitrate aqueous solution at a temperature of 35 °C for 2 h. The weight ratio of the zinc nitrate aqueous solution to the unbonded Y molecular sieve was 6:1. After drying at 120 °C for 12 h, a solid product was obtained.
[0118] d) Take 10g of the solid product and immerse it in an aqueous solution of 15g Ce(NO3)3 and Co(NO3)2, where the mass concentrations of Ce(NO3)3 and Co(NO3)2 are 7.5% and 5%, respectively. Dry the mixture at 150℃ for 8 hours, then calcine it at 500℃ for 7 hours to obtain the modified Y molecular sieve, whose size is basically the same as that of the Y molecular sieve precursor. The specific composition is shown in Table 1. Its lateral compressive strength was measured to be 145 N / cm.
[0119] Example 3
[0120] a) After solid-liquid separation, water washing and drying, the slurry from step a in Example 1 was used to obtain Y molecular sieve seed crystals, and the SiO2 content was measured to be 70%.
[0121] b) Preparation of binder-free Y molecular sieve precursor: 5.3g of the above-mentioned Y molecular sieve seed crystals, 15.6g of silica, 75.2g of alkaline silica sol (SiO2 content of 40wt%), 23.1g of aluminum nitrate, 0.9g of Tianqing powder, and 18.2g of 7wt% nitric acid aqueous solution were mixed evenly. The SiO2 / Al2O3 ratio in the mixture was 6. The mixture was extruded to obtain cylindrical strips with a diameter of 5mm, and then cut into particles with a length of 9-13mm. The particles were dried at 150℃ for 6h.
[0122] c) Place 10g of the Y molecular sieve precursor obtained above into 15g of 2wt% NaOH aqueous solution, place it in a microwave reactor, heat to 75℃, and crystallize at a microwave power of 500W for 5h. Then perform solid-liquid separation and washing to obtain a non-bonded Y molecular sieve with a relative crystallinity of 98.9%.
[0123] d) The unbonded Y molecular sieve was exchanged twice with a 1 mol / L zinc nitrate aqueous solution at a temperature of 45℃ for 3 h. The weight ratio of zinc nitrate aqueous solution to unbonded Y molecular sieve was 8:1. After drying at 120℃ for 10 h, a solid product was obtained.
[0124] e) Take 10g of the solid product and immerse it in an aqueous solution of 15g Ce(NO3)3 and Co(NO3)2, where the mass concentrations of Ce(NO3)3 and Co(NO3)2 are 6.2% and 4%, respectively. Dry the mixture at 150℃ for 8 hours, then calcine it at 500℃ for 6 hours to obtain the modified Y molecular sieve, whose size is basically the same as that of the Y molecular sieve precursor. The specific composition is shown in Table 1. Its lateral compressive strength was measured to be 140 N / cm.
[0125] Example 4
[0126] The method of Example 2 was followed, except that Ce(NO3)3 in step d) was replaced with La(NO3)3 at a mass concentration of 3%, resulting in modified Y molecular sieves. The specific composition is shown in Table 1. Its lateral compressive strength was measured to be 147 N / cm.
[0127] Example 5
[0128] The procedure was carried out according to Example 1, except that Co(NO3)2 in step e) was replaced with Ni(NO3)2 at a mass concentration of 9%. Modified Y molecular sieve was obtained, with dimensions essentially the same as the Y molecular sieve precursor. The specific composition is shown in Table 1. Its lateral compressive strength was measured to be 138 N / cm.
[0129] Example 6
[0130] The method was followed according to Example 1, except that the number of exchanges in step d) was changed to one, resulting in a modified Y molecular sieve with dimensions essentially the same as the Y molecular sieve precursor. The specific composition is shown in Table 1. Its lateral compressive strength was measured to be 132 N / cm.
[0131] Example 7
[0132] The method of Example 3 was followed, except that the amount of aluminum nitrate used in step b) was 13.5 g, resulting in modified Y molecular sieve with dimensions essentially the same as the Y molecular sieve precursor. The specific composition is shown in Table 1. Its lateral compressive strength was measured to be 136 N / cm.
[0133] Comparative Example 1
[0134] The method was followed as in Example 1, except that microwave crystallization in step c) was replaced with conventional hydrothermal crystallization, while the crystallization temperature and time remained unchanged, resulting in a modified Y molecular sieve with dimensions essentially the same as the Y molecular sieve precursor. The specific composition is shown in Table 1. Its lateral compressive strength was measured to be 85 N / cm.
[0135] Comparative Example 2
[0136] The procedure was carried out according to Example 1, except that the diameter of the cylindrical strip obtained by extrusion molding in step b) was 2 mm, while the other steps remained unchanged, resulting in a modified Y molecular sieve with dimensions essentially the same as the Y molecular sieve precursor. The specific composition is shown in Table 1. Its lateral compressive strength was measured to be 96 N / cm.
[0137] Comparative Example 3
[0138] The method of Example 1 was followed, except that the crystallization temperature of the microwave crystallization step in step c) was set to 80°C, resulting in an unbound Y molecular sieve with a relative crystallinity of 95.1%. Other steps remained unchanged, yielding a modified Y molecular sieve with dimensions essentially the same as the Y molecular sieve precursor. The specific composition is shown in Table 1. Its lateral compressive strength was measured to be 125 N / cm.
[0139] Comparative Example 4
[0140] The procedure was carried out according to Example 1, except that step d) was omitted, while the other steps remained unchanged, to obtain a modified Y molecular sieve. The size of this modified sieve was essentially the same as that of the Y molecular sieve precursor. The specific composition is shown in Table 1. Its lateral compressive strength was measured to be 130 N / cm.
[0141] Table 1
[0142]
[0143] Note: All contents mentioned in Table 1 are by weight, and the unit is weight %
[0144] Test Example 1
[0145] The modified Y molecular sieve denitrifying agent prepared in the examples and comparative examples was used to remove nitrogen-containing alkaline substances from benzene. 1g of the denitrifying agent was placed in a fixed-bed reactor. A benzene solution of pyridine (total nitrogen content 10mg / L) was passed through the reaction bed at a mass hourly space velocity of 30mL / g / h under the conditions of 80℃ and 0.2MPa. Samples were taken every 2 hours, and the N content was detected by a sulfur-nitrogen analyzer. The results are shown in Table 2. When the nitrogen-containing alkaline substance content is above 0.1mg / L, it is considered that the denitrifying agent has been penetrated.
[0146] The breakthrough curve of the denitrifying agent containing the modified Y molecular sieve prepared in Example 1 is given as an example. Figure 2 As shown, after 40 hours of operation, when the nitrogen content in benzene exceeds 0.1 mg / L, the amount of nitrogen adsorbed through the denitrifying agent is 12 mg / g.
[0147] Table 2
[0148]
[0149] Breakthrough nitrogen adsorption capacity (mg / g) = Runtime to reach breakthrough nitrogen adsorption capacity (h) × Mass hourly space velocity (mL / g / h) × Total nitrogen content (mg / L)
[0150] As can be seen from the results in Table 2, the denitrifying agent containing the modified Y molecular sieve of the present invention has a significantly better denitrification effect.
[0151] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A modified Y molecular sieve, characterized in that, The modified Y molecular sieve contains Y molecular sieve, ZnO, lanthanide metal oxides, iron metal oxides, and optional binders; Based on the total weight of the modified Y molecular sieve, the content of Y molecular sieve is 60-80% by weight, the content of ZnO is 10-25% by weight, the content of lanthanide metal oxides is 2-10% by weight, the content of iron metal oxides is 2-10% by weight, and the content of binder is less than 2% by weight. The method for preparing the modified Y molecular sieve includes the following steps: 1) Y seed crystals, aluminum source, silicon source, adhesive solvent and optional pore-forming agent are kneaded together to obtain binder-free Y molecular sieve precursor; 2) The binderless Y molecular sieve precursor is subjected to liquid-phase crystallization under microwave conditions. In the crystallization product, the relative crystallinity of the binderless Y molecular sieve is above 98%. 3) Exchange the binder-free Y molecular sieve obtained in step 2) with an aqueous solution containing zinc compounds; 4) Load the solid product obtained in step 3) with lanthanide and iron-based metal compounds to obtain modified Y molecular sieve.
2. The modified Y molecular sieve according to claim 1, wherein, Based on the total weight of the modified Y molecular sieve, the content of Y molecular sieve is 65-75% by weight, the content of ZnO is 15-22% by weight, the content of lanthanide metal oxides is 2-8% by weight, and the content of iron metal oxides is 2-8% by weight.
3. The modified Y molecular sieve according to claim 1, wherein, The weight ratio of ZnO, lanthanide metal oxides, and iron metal oxides is 1:0.05-0.5:0.05-0.
4.
4. The modified Y molecular sieve according to claim 3, wherein, The weight ratio of ZnO, lanthanide metal oxides, and iron metal oxides is 1:0.1-0.35:0.1-0.
3.
5. The modified Y molecular sieve according to claim 1, wherein, The Na2O content in the modified Y molecular sieve is less than 2% by weight.
6. The modified Y molecular sieve according to any one of claims 1-5, wherein, The modified Y molecular sieve has a cross-sectional diameter of 3.5-7 mm and a length of 5-50 mm.
7. The modified Y molecular sieve according to claim 6, wherein, The modified Y molecular sieve has a cross-sectional diameter of 4-6.5 mm and a length of 7-25 mm.
8. The modified Y molecular sieve according to any one of claims 1-5, wherein, The lateral compressive strength of the modified Y molecular sieve is 125-170 N / cm.
9. The modified Y molecular sieve according to claim 8, wherein, The lateral compressive strength of the modified Y molecular sieve is 125-150 N / cm.
10. The modified Y molecular sieve according to any one of claims 1-5, wherein, The SiO2 / Al2O3 molar ratio of the modified Y molecular sieve is 5-20.
11. The modified Y molecular sieve according to claim 10, wherein, The SiO2 / Al2O3 molar ratio of the modified Y molecular sieve is 5-10.
12. The modified Y molecular sieve according to any one of claims 1-5, wherein, The lanthanide metal is La and / or Ce; The iron-based metal is Ni and / or Co.
13. A method for preparing modified Y molecular sieve, the method comprising the following steps: 1) Y seed crystals, aluminum source, silicon source, adhesive solvent and optional pore-forming agent are kneaded together to obtain binder-free Y molecular sieve precursor; 2) The binderless Y molecular sieve precursor is subjected to liquid-phase crystallization under microwave conditions. In the crystallization product, the relative crystallinity of the binderless Y molecular sieve is above 98%. 3) Exchange the binder-free Y molecular sieve obtained in step 2) with an aqueous solution containing zinc compounds; 4) Load the solid product obtained in step 3) with lanthanide and iron-based metal compounds to obtain modified Y molecular sieve.
14. The method according to claim 13, wherein, The amounts of zinc compounds, lanthanide metal compounds, and iron metal compounds used in the prepared modified Y molecular sieve are such that, based on the total weight of the modified Y molecular sieve, the content of Y molecular sieve is 60-80% by weight, the content of ZnO is 10-25% by weight, the content of lanthanide metal oxides is 2-10% by weight, and the content of iron metal oxides is 2-10% by weight.
15. The method according to claim 14, wherein, The amounts of zinc compounds, lanthanide metal compounds, and iron metal compounds used in the prepared modified Y molecular sieve are such that, based on the total weight of the modified Y molecular sieve, the content of Y molecular sieve is 65-75% by weight, the content of ZnO is 15-22% by weight, the content of lanthanide metal oxides is 2-8% by weight, and the content of iron metal oxides is 2-8% by weight.
16. The method according to claim 13, wherein, The amount of zinc-containing compounds, lanthanide metal compounds, and iron-based metal compounds used results in a weight ratio of ZnO, lanthanide metal oxides, and iron-based metal oxides of 1:0.05-0.5:0.05-0.4 in the prepared modified Y molecular sieve.
17. The method according to claim 13, wherein, The amount of zinc-containing compounds, lanthanide metal compounds, and iron-based metal compounds used results in a weight ratio of ZnO, lanthanide metal oxides, and iron-based metal oxides of 1:0.1-0.35:0.1-0.3 in the prepared modified Y molecular sieve.
18. The method according to claim 13, wherein, Step 1) The forming process is extrusion forming.
19. The method according to claim 13, wherein, The cross-sectional diameter of the binderless Y molecular sieve precursor is 3.5-7 mm; the length is 5-50 mm.
20. The method according to claim 19, wherein, The cross-sectional diameter of the binderless Y molecular sieve precursor is 4-6.5 mm; the length is 7-25 mm.
21. The method according to claim 13, wherein, Based on the total SiO2 weight in the binderless Y molecular sieve precursor, the SiO2 weight content in the Y seed crystal is 1-15%.
22. The method according to claim 21, wherein, Based on the total SiO2 weight in the binderless Y molecular sieve precursor, the SiO2 weight content in the Y seed crystal is 5-10%.
23. The method according to claim 13, wherein, The molar ratio of silicon source to aluminum source is 5-20:1, wherein the silicon source is SiO2 and the aluminum source is Al2O3.
24. The method according to claim 23, wherein, The molar ratio of silicon source to aluminum source is 5-10:1, wherein the silicon source is SiO2 and the aluminum source is Al2O3.
25. The method according to claim 13, wherein, The aluminum source is a soluble salt of aluminum.
26. The method of claim 25, wherein, The aluminum source is selected from at least one of aluminum sulfate, aluminum nitrate, and aluminum acetate.
27. The method according to claim 13, wherein, The silicon source is selected from at least one of silicon powder, silica, and silica sol.
28. The method according to any one of claims 13-27, wherein, In the crystallized products, the relative crystallinity of binder-free Y molecular sieve is 98-100%.
29. The method according to any one of claims 13-27, wherein, Step 2) describes liquid-phase crystallization under microwave conditions, which includes mixing a binder-free Y molecular sieve precursor and an alkaline solution and then crystallizing the mixture under microwave conditions.
30. The method according to any one of claims 13-27, wherein, The crystallization conditions include: a temperature of 40-100℃; a time of 0.15-12 hours; and a microwave power of 100-900W.
31. The method according to claim 30, wherein, The crystallization conditions include: a temperature of 60-95℃; a time of 1-8 hours; and a microwave power of 300-700 W.
32. The method according to claim 29, wherein, The weight ratio of the alkaline solution to the binder-free Y molecular sieve precursor is 0.8-3:
1.
33. The method according to claim 32, wherein, The weight ratio of the alkaline solution to the binder-free Y molecular sieve precursor is 1.1-2:
1.
34. The method according to claim 29, wherein, The concentration of the alkaline solution is 1-5 wt%; The alkali is selected from at least one of NaOH, KOH and CsOH.
35. The method according to any one of claims 13-27, wherein, The conditions for the exchange include: a temperature of 30-70℃ and a time of 1-10 h.
36. The method according to claim 35, wherein, The exchange conditions include: a temperature of 35-60℃ and a time of 2-5 hours.
37. The method according to any one of claims 13-27, wherein, The number of exchanges is 1-5.
38. The method according to claim 37, wherein, The number of exchanges is 2-4.
39. The method according to any one of claims 13-27, wherein, The weight ratio of the aqueous solution containing the zinc compound to the binderless Y molecular sieve is 3-20:
1.
40. The method according to claim 39, wherein, The weight ratio of the aqueous solution containing the zinc compound to the binderless Y molecular sieve is 5-10:
1.
41. The method according to any one of claims 13-27, wherein, The concentration of the aqueous solution containing the zinc compound is 0.5-2 mol / L; The zinc-containing compound is a soluble salt of zinc.
42. The method according to claim 41, wherein, The zinc-containing compound is Zn(NO3)2 and / or ZnCl2.
43. The method according to any one of claims 13-27, wherein, The lanthanide metal is La and / or Ce; The iron-based metal is Ni and / or Co.
44. The method according to any one of claims 13-27, wherein, The lanthanide metal compound is a soluble salt of a lanthanide metal; the iron metal compound is a soluble salt of an iron metal.
45. The method according to claim 44, wherein, The lanthanide metal compound is selected from at least one of cerium nitrate, cerium chloride, lanthanum nitrate, and lanthanum chloride; The iron-based metal compound is selected from at least one of cobalt nitrate, cobalt chloride, nickel nitrate, and nickel chloride.
46. The method according to any one of claims 13-27, wherein, The method further includes: calcining the loaded lanthanide and iron-based metal compounds as described in step 4); The roasting conditions include: a temperature of 450-600℃ and a time of 2-12 hours.
47. The method according to claim 46, wherein, The roasting conditions include: a temperature of 500-550℃ and a time of 4-8 hours.
48. The use of the modified Y molecular sieve according to any one of claims 1-12 or the modified Y molecular sieve prepared by any one of claims 13-47 in denitrification.
49. The application according to claim 48, wherein, Application of the modified Y molecular sieve in the removal of nitrogen-containing alkaline substances from benzene.
50. A method for removing nitrogen-containing alkaline substances from benzene, the method comprising: Benzene containing nitrogen-based alkaline substances is contacted with a denitrifying agent, wherein the denitrifying agent comprises the modified Y molecular sieve according to any one of claims 1-12 or the modified Y molecular sieve prepared by the method according to any one of claims 13-47.
51. The method according to claim 50, wherein, In the material obtained from the contact, the nitrogen-containing alkaline substances were reduced to below 0.1 mg / L based on the total nitrogen content.
52. The method according to claim 50, wherein, The contact conditions include: a temperature of 40-200℃; a pressure of 0.1-2 MPa; and a mass hourly space velocity of 10-60 mL / g / h.
53. The method according to claim 52, wherein, The contact conditions include: a temperature of 60-160℃; a pressure of 0.5-1 MPa; and a mass hourly space velocity of 20-45 mL / g / h.
54. The method according to claim 50, wherein, The content of the nitrogen-containing alkaline substance is 1-50 mg / L.
55. The method according to claim 54, wherein, The content of the nitrogen-containing alkaline substance is 5-15 mg / L.
56. The method of claim 50, wherein, The nitrogen-containing basic substance includes at least one of pyridine, quinoline, and aniline.
Citation Information
Patent Citations
C4 hydrocarbon deep desulfurization method and thiol and disulfide removal agent used therein
CN101591213A
Preparation method of binderless Y molecular sieve catalyst
CN107511162A
Continuous process for preparing ethylbenzene using liquid phase alkylation and vapour phase transalkylation
CN1171096A
Catalyst for liquid phase alkylation of ethylene to prepare ethylbenzene
CN1506340A
Liquid phase alkylation or transalkylation process using zeolite beta
US4891458A