An in-situ self-generated (Al3Ti-AlN-TiN) multi-scale reinforced Al-based composite material and its hot-pressing preparation method.
By employing a hot-pressing method for preparing in-situ self-generated (Al₃Ti-AlN-TiN) multi-phase multi-scale reinforced Al-based composite materials, the problems of poor bonding between the reinforcement and the matrix and dimensional inhomogeneity have been solved, enabling the preparation of high-performance aluminum-based composite materials suitable for multiple industrial fields.
Patent Information
- Application Number
- CN202410069920.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-17
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-01-17
AI Technical Summary
In existing aluminum matrix composites, the bonding between the reinforcement and the matrix is poor, and the size of the in-situ self-generated reinforcement is uneven, making it difficult to control at high temperatures and affecting the overall performance of the composite material.
A hot-pressing method for preparing in-situ self-generated (Al₃Ti-AlN-TiN) multi-scale reinforced Al matrix composites was adopted. Through ball milling, cold pressing and hot-pressing sintering processes, the dissociation and topological transformation of Ti₂AlN were controlled under a high-purity argon atmosphere to generate submicron-sized AlN, TiN and Al₃Ti, which were uniformly distributed in the matrix.
It achieves high flexural strength, compressive strength and fracture toughness in aluminum-based composite materials, and has the properties of being lightweight, high-strength and high-toughness, making it suitable for automotive, military and aerospace fields.
Smart Images

Figure CN117926060B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to an in-situ self-generated (Al3Ti-AlN-TiN) multi-phase multi-scale reinforced Al-based composite material and its hot-pressing preparation method. Background Technology
[0002] Aluminum-based composites, with their outstanding advantages such as low density, high specific strength, and high plasticity, meet the industry's demand for "lightweighting" and have broad application prospects in the automotive, military, and aerospace fields. However, conventional reinforcements often suffer from poor bonding with the matrix (SiC, Al2O3, etc.) or self-agglomeration (graphene, carbon nanotubes, etc.), which greatly impair the overall performance of the composites. Currently, there are methods to overcome these problems by adding precursors and synthesizing new reinforcements in situ through reactions during the preparation process. However, this method often struggles to control the size and distribution of the in-situ self-generated reinforcements. Al3Ti, as a widely used in-situ self-generated intermetallic compound, exhibits high temperature sensitivity, causing it to easily grow along orientation at high temperatures, which greatly limits its application. To improve this situation, it is necessary to find suitable methods to inhibit the growth of Al3Ti.
[0003] Ti₂AlN is a ternary layered compound ceramic possessing both covalent and metallic bonds. It exhibits high electrical and thermal conductivity similar to metallic materials, along with certain high-temperature plasticity, while also possessing the high modulus, low density, and excellent tribological properties of ceramics. At high temperatures, the Ti and N atoms in Ti₂AlN gradually dissociate, forming Al₃Ti and AlN with Al, and undergoing topological transformations to become smaller TiN compounds, all of which are highly promising reinforcements.
[0004] The application of Al3Ti, AlN, or TiN as reinforcements in aluminum has been reported, but this is usually done by direct external addition to the matrix. This method has significant drawbacks: First, the poor interfacial bonding between the added ceramic / intermetallic compound and the matrix is an inherent problem in the preparation of composites using the external method. Second, if the reinforcement is obtained through in-situ self-generation, the composite preparation temperature is generally high, causing the temperature-sensitive Al3Ti to grow along its habit plane, resulting in a larger size and affecting the strengthening effect. Furthermore, obtaining all three reinforcements simultaneously requires different amounts if using the external method, as this often necessitates a low addition amount to ensure the composite's density, and preventing agglomeration in the matrix becomes a challenge. Even with the in-situ self-generation method, balancing the significantly different generation temperatures of the three reinforcements to obtain a multiphase reinforced composite with suitable size and uniform distribution is also a major difficulty. Therefore, there are currently no reports of applying Ti2AlN to aluminum in an in-situ self-generated multiphase reinforced composite. Summary of the Invention
[0005] In view of this, the purpose of this invention is to provide a simple and low-cost hot pressing method for preparing in-situ self-generated (Al3Ti-AlN-TiN) multi-scale reinforced Al-based composite materials.
[0006] The present invention also aims to provide an in-situ self-generated (Al3Ti-AlN-TiN) multi-scale reinforced Al-based composite material.
[0007] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:
[0008] According to a first aspect of the present invention, a hot pressing method for preparing in-situ self-generated (Al3Ti-AlN-TiN) multi-scale reinforced Al-based composite materials is provided, comprising the following steps:
[0009] Step S1, prepare the materials according to the volume fraction of the composite material: weigh Ti2AlN powder and Al powder according to the volume ratio, wherein the Ti2AlN content is 5-20 vol.%, and the remainder is Al powder;
[0010] Step S2: Place the various raw materials weighed in step S1 into a ball mill and ball mill them for 10 hours at a speed of 90 r / min according to a ball-to-material ratio of 5:1.
[0011] Step S3: The mixed powder is placed on the bottom of a graphite mold coated with boron nitride, with a thickness of 10-20 mm, and cold-pressed at 15 MPa to obtain the blank.
[0012] Step S4: Sintering is performed under a high-purity argon atmosphere at a temperature of 660–770°C, a heating rate of 10°C / min, and a holding time of 30 min. Subsequently, the furnace is cooled to 590–630°C, pressurized to 30 MPa, and held at that temperature and pressure for 30 min. Finally, the furnace is cooled to 400°C and the pressure is released to obtain the final product. According to a second aspect of the present invention, an in-situ self-generated (Al3Ti-AlN-TiN) multi-scale reinforced Al-based composite material prepared by the preparation method of any embodiment of the first aspect is provided.
[0013] The above-described technical solution of the present invention has at least one of the following beneficial effects:
[0014] According to the preparation method of the present invention, Al3Ti and AlN are generated in situ by the chemical reaction of Ti and N atoms dissociated from Ti2AlN at high temperature with the Al matrix; the topological transformation of Ti2AlN is achieved by TiN, and Al3Ti further reacts with N interstitial in the matrix to generate TiN. The reaction of Al3Ti at high temperature, along with the dispersed TiN and AlN in the matrix, effectively refines Al3Ti, inhibits its orientation growth, and also refines the matrix grains. Due to the high nucleation energy of AlN, its size is only 290–632 nm. Therefore, AlN, TiN (328–600 nm), and Al3Ti (0.98–3.85 μm) together form a submicron-scale multi-scale complex phase synergistic strengthening effect on the matrix.
[0015] According to the preparation method of this invention, the in-situ self-generated (Al3Ti-AlN-TiN) multi-scale reinforced Al-based composite material has a maximum flexural strength of 640 MPa, a maximum compressive strength of 782 MPa, and a maximum fracture toughness of 14.98 MPa·m. 1 / 2 The batching method used in this invention can also be applied to techniques such as stir casting and powder metallurgy, obtaining aluminum-based composite materials with good comprehensive properties over a wide temperature range. The preparation method of this invention has significant advantages such as simple process, convenient operation, and low cost.
[0016] The in-situ self-generated (Al3Ti-AlN-TiN) multi-scale reinforced Al-based composite material of the present invention has the properties of being lightweight, high-strength, and high-toughness. It can open up new paths for the research and development and preparation of advanced aluminum-based composite materials with adjustable morphology and mechanical strength, and can be widely used in many fields such as automobiles, military industry, and aerospace. Attached Figure Description
[0017] Figure 1 A scanning electron microscope image of an in-situ self-generated (Al3Ti-AlN-TiN) multi-scale reinforced Al-based composite material is shown.
[0018] Figure 2 The energy spectrum results of TiN and AlN under online and spot scan modes are shown.
[0019] Figure 3 The XRD pattern of the in-situ self-generated (Al3Ti-AlN-TiN) multi-phase multi-scale reinforced Al-based composite material is shown. Detailed Implementation
[0020] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the described embodiments of the present invention are within the scope of protection of the present invention.
[0021] The following describes in detail the preparation method of in-situ self-generated (Al3Ti-AlN-TiN) multi-scale reinforced Al-based composite material according to an embodiment of the present invention.
[0022] The preparation method of in-situ self-generated (Al3Ti-AlN-TiN) multi-scale reinforced Al-based composite material according to an embodiment of the present invention includes the following steps:
[0023] Step S1, prepare the materials according to the volume fraction of the composite material: weigh Ti2AlN powder and Al powder according to the volume ratio, wherein the Ti2AlN content is 5-20 vol.%, and the remainder is Al powder;
[0024] Step S2: Place the various raw materials weighed in step S1 into a ball mill and ball mill them for 10 hours at a speed of 90 r / min according to a ball-to-material ratio of 5:1.
[0025] Step S3: The mixed powder is placed on the bottom of a graphite mold coated with boron nitride, with a thickness of 10-20 mm, and cold-pressed at 15 MPa to obtain the blank.
[0026] Step S4: Sintering is carried out in a high-purity argon atmosphere at a sintering temperature of 660–770°C, a heating rate of 10°C / min, and a holding time of 30 min. Then, the furnace is cooled to 590–630°C, pressurized to 30 MPa, and held at the same temperature and pressure for 30 min. Finally, the furnace is cooled to 400°C and the pressure is released to obtain the final product.
[0027] The preparation method according to the present invention and the in-situ self-generated (Al3Ti-AlN-TiN) multi-scale reinforced Al-based composite material obtained therefrom are further described below with reference to specific embodiments. The flexural strength test method refers to GB / T6569-1986, the compressive strength test method refers to JIS R 1608-200, and the fracture toughness test method refers to GB / T 23806-2009.
[0028] Example 1
[0029] (1) Weigh 4.6g of Ti2AlN powder and 26.2g of Al powder into a ball mill jar according to a Ti2AlN to Al volume ratio of 10:90. Add agate balls at a ball-to-material ratio of 5:1. Place the ball mill jar on a drum ball mill and ball mill at a speed of 90r / min for 10h to ensure that the powder is fully mixed and uniform.
[0030] (2) Place the ball-milled powder into a graphite mold coated with boron nitride and cold press it at 15 MPa.
[0031] (3) Sintering was carried out using hot pressing sintering. The specific process was as follows: under a high-purity argon atmosphere, the temperature was increased to 660℃ at a rate of 10℃ / min, pressure was applied to 30MPa, and the temperature and pressure were held for 30min, followed by cooling to 400℃ in the furnace to release the pressure. (Al3Ti-AlN-TiN) / Al was obtained, wherein the Al3Ti content was 21.60 vol.%, with a size of 0.98 μm; the TiN content was 3.59 vol.%, with a size of 328 nm; the AlN content was 1.32 vol.%, with a size of 290 nm; and the remainder was Al. The composite material was tested for performance: flexural strength was 400.00±3.15 MPa, compressive strength was 306.83±6.31 MPa, and fracture toughness was 9.20±0.51 MPa·m. 1 / 2 .
[0032] Example 2
[0033] (1) Weigh 2.3g of Ti2AlN powder and 27.7g of Al powder into a ball mill jar according to a Ti2AlN to Al volume ratio of 5:95. Add agate balls at a ball-to-material ratio of 5:1. Place the ball mill jar on a roller ball mill and ball mill at a speed of 90r / min for 10h to ensure that the powder is fully mixed and uniform.
[0034] (2) Place the ball-milled powder into a graphite mold coated with boron nitride and cold press it at 15 MPa.
[0035] (3) Sintering was carried out using hot pressing sintering. The specific process was as follows: under a high-purity argon atmosphere, the temperature was raised to 730℃ at a rate of 10℃ / min, held for 30min, then cooled to 590℃ in the furnace, pressurized to 30MPa, held for 30min, and then cooled to 400℃ in the furnace to release the pressure. (Al3Ti-AlN-TiN) / Al was obtained, wherein the Al3Ti content was 12.70 vol.%, with a size of 3.85 μm; the TiN content was 5.92 vol.%, with a size of 500 nm; the AlN content was 2.57 vol.%, with a size of 632 nm; and the remainder was Al. The composite material was tested for performance: flexural strength was 395.90±4.12 MPa, compressive strength was 263.12±5.90 MPa, and fracture toughness was 10.42±0.46 MPa·m.1 / 2 .
[0036] Example 3
[0037] (1) Weigh 4.6g of Ti2AlN powder and 26.2g of Al powder into a ball mill jar according to a Ti2AlN to Al volume ratio of 10:90. Add agate balls at a ball-to-material ratio of 5:1. Place the ball mill jar on a drum ball mill and ball mill at a speed of 90r / min for 10h to ensure that the powder is fully mixed and uniform.
[0038] (2) Place the ball-milled powder into a graphite mold coated with boron nitride and cold press it at 15 MPa.
[0039] (3) Sintering was performed using a hot-pressing sintering method. The specific process was as follows: Under a high-purity argon atmosphere, the temperature was raised to 770℃ at a rate of 10℃ / min, held for 30min, then cooled to 600℃ in the furnace, pressurized to 30MPa, held for 30min, and then cooled to 400℃ in the furnace to release the pressure. This yielded (Al3Ti-AlN-TiN) / Al, where Al3Ti content was 38.70 vol.%, with a size of 3.66 μm; TiN content was 21.02 vol.%, with a size of 574 nm; AlN content was 9.95 vol.%, with a size of 470 nm; and the remainder was Al. The composite material was tested for performance: flexural strength was 426.48 ± 5.82 MPa, compressive strength was 442.84 ± 5.63 MPa, and fracture toughness was 13.58 ± 1.43 MPa·m. 1 / 2 .
[0040] Example 4
[0041] (1) Weigh 9.24g of Ti2AlN powder and 23.3g of Al powder into a ball mill jar according to a Ti2AlN to Al volume ratio of 20:90. Add agate balls at a ball-to-material ratio of 5:1. Place the ball mill jar on a drum ball mill and ball mill at a speed of 90r / min for 10h to ensure that the powder is fully mixed and uniform.
[0042] (2) Place the ball-milled powder into a graphite mold coated with boron nitride and cold press it at 15 MPa.
[0043] (3) Sintering was performed using a hot-pressing sintering method. The specific process was as follows: Under a high-purity argon atmosphere, the temperature was raised to 770℃ at a rate of 10℃ / min, held for 30min, then cooled to 630℃ in the furnace, pressurized to 30MPa, held for 30min, and then cooled to 400℃ in the furnace to release the pressure. This yielded (Al3Ti-AlN-TiN) / Al, where Al3Ti content was 39.97 vol.%, with a size of 3.42 μm; TiN content was 35.55 vol.%, with a size of 600 nm; AlN content was 11.01 vol.%, with a size of 338 nm; and the remainder was Al. The composite material was tested for performance: flexural strength was 635.18 ± 5.79 MPa, compressive strength was 776.21 ± 6.37 MPa, and fracture toughness was 9.82 ± 1.09 MPa·m. 1 / 2 .
[0044] The above description represents the preferred embodiments of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. An in-situ self-generated (Al3Ti-AlN-TiN) multi-phase multi-scale reinforced Al-based composite material, characterized in that: (1) The raw materials are Ti2AlN powder and Al powder, wherein the content of Ti2AlN is 5~20 vol.%, and the remainder is Al; (2) Ti and N atoms of Ti2AlN react with Al to generate Al3Ti and AlN in situ; Ti2AlN undergoes topological transformation and Al3Ti reacts with interstitial N at high temperature to generate TiN, forming an in situ self-generated (Al3Ti-TiN-AlN) multiphase synergistic reinforced aluminum matrix composite material; the content of in situ self-generated Al3Ti is 12.70~39.97 vol.%, with a size distribution of 0.98~3.85 μm; the content of TiN is 3.59~35.55 vol.%, with a size distribution of 328~600 nm; the content of AlN is 1.32~11.01 vol.%, with a size distribution of 290~632 nm; the remainder is the Al matrix; the in situ self-generated micron-sized Al3Ti, nano-sized TiN and AlN are dispersed in the matrix and are firmly bonded to the matrix interface.
2. The hot-pressing preparation method of (Al3Ti-AlN-TiN) multi-phase multi-scale reinforced Al-based composite material according to claim 1, characterized in that, Includes the following steps: Step S1, prepare the materials according to the volume fraction of the composite material: weigh Ti2AlN powder and Al powder according to the volume ratio, wherein the Ti2AlN content is 5~20 vol.%, and the remainder is Al powder; Step S2: Place the various raw materials weighed in step S1 into a ball mill and ball mill them for 10 hours at a speed of 90 r / min according to a ball-to-material ratio of 5:
1. Step S3: The mixed powder is placed on the bottom of a graphite mold coated with boron nitride, with a thickness of 10-20 mm, and then cold-pressed at 15 MPa to obtain a green body. Step S4: Sintering is carried out in a high-purity argon atmosphere at a sintering temperature of 660~770 ℃, a heating rate of 10 ℃ / min, and a holding time of 30 min; then the furnace is cooled to 590~630 ℃, pressurized to 30 MPa, and held at the temperature and pressure for 30 min; the furnace is then cooled to 400 ℃ and the pressure is released to obtain the final product.
Citation Information
Patent Citations
Preparation method for in-situ aluminium base composite material inoculant
CN102864343A
Powder metallurgy preparation method of double-reinforcement-phase high-chromium cast iron wear-resistant composite material
CN115029606A