High-strength self-lubricating bearing material and preparation method thereof

By mixing and sintering aluminum powder, nickel powder, copper-clad iron powder, and MoS₂ powder with copper powder in specific proportions, the problem of high porosity in copper-based sliding bearings during sintering was solved, resulting in a self-lubricating bearing material with high strength and excellent mechanical properties, suitable for specific mechanical equipment.

CN117926069BActive Publication Date: 2026-11-20CHONGQING THREE GORGES UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311190618.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-15
Publication Date
2026-11-20
Estimated Expiration
2043-09-15

AI Technical Summary

Technical Problem

Existing powder metallurgy methods for preparing copper-based sliding bearings result in high porosity during sintering, leading to low material strength and susceptibility to cracking or collapse, thus failing to meet the requirements for high strength and excellent mechanical properties.

Method used

A high-strength self-lubricating bearing material is prepared by mixing aluminum powder, nickel powder, copper-clad iron powder, and MoS₂ powder with copper powder in a specific ratio, followed by powder mixing, pressing, and sintering processes, thereby controlling porosity and improving material strength.

Benefits of technology

The prepared high-strength self-lubricating bearing material has low sintering density, high yield strength, and good wear resistance. It is suitable for service environments where lubrication is not possible and is widely used in steel, metallurgy, and agricultural machinery equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The application discloses a kind of high-strength self-lubricating bearing materials and preparation method thereof, wherein, high-strength self-lubricating bearing material includes the following weight percentage of component raw materials: 10% aluminum powder, 4% nickel powder, 6% copper-coated iron powder, 4%~8% MoS2 powder, the balance is copper powder.The high-strength self-lubricating bearing material of the application has the advantages of low relative sintering density, high yield strength, good wear resistance, etc.;The preparation method of the high-strength self-lubricating bearing material of the application has the advantages of easy to obtain raw materials, low cost, simple process, good parameter control, can be used in the production of sliding bearing on a large scale, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of self-lubricating materials technology, and in particular to a high-strength self-lubricating bearing material and its preparation method. Background Technology

[0002] Bearings are essential components in various types of mechanical equipment in modern times, and their performance directly affects and determines the performance of the equipment. Based on the form of friction during operation, they are divided into two main categories: rolling bearings and sliding bearings. Rolling bearings experience rolling friction during rotation, while sliding bearings experience surface-to-surface sliding friction. Sliding bearings are characterized by high speed, stable operation, good vibration resistance, high load-bearing capacity, low noise, and long service life, and are widely used in machinery manufacturing, large power plants, integrated steel enterprises, and integrated chemical enterprises. Self-lubricating sliding bearing materials achieve self-lubrication by adding powdered solid lubricants to copper-based materials, or by adding liquid lubricating oil before use, while requiring little or no lubrication during operation.

[0003] Sliding bearings are manufactured using powder metallurgy, which offers advantages such as resource conservation, material saving, and optimized performance. However, copper-based sliding bearings prepared using powder metallurgy undergo expansion during sintering, leading to increased porosity, decreased sintering density, and low material strength. This results in a tendency for the material to crack or collapse during practical use. Therefore, there is an urgent need to develop self-lubricating bearing materials with high porosity and excellent mechanical properties. Summary of the Invention

[0004] In view of the shortcomings of the prior art, the technical problem to be solved by the present invention is: how to provide a high-strength self-lubricating bearing material with high porosity, high strength and superior mechanical properties and its preparation method.

[0005] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: A high-strength self-lubricating bearing material is characterized by comprising the following raw materials in weight percentage: 8%–11% aluminum powder, 3%–5% nickel powder, 5%–10% copper-clad iron powder, 4%–8% MoS2 powder, with the balance being copper powder.

[0006] As an optimization, the weight percentage of the MoS2 powder is 6%.

[0007] As an optimization, the weight percentage of aluminum powder is 10%, the weight percentage of nickel powder is 4%, and the weight percentage of copper-clad iron powder is 6%.

[0008] A method for preparing a high-strength self-lubricating bearing material, characterized by comprising the following steps: S1. First, obtain the raw materials according to the following weight percentages: 8% to 11% aluminum powder, 3% to 5% nickel powder, 5% to 10% copper-clad iron powder, 4% to 8% MoS2 powder, and the remainder is copper powder. S2. Mixing: Put the raw materials obtained in step S1 into a grinding mill and mix for 1 to 6 hours; S3. Pressing: Press the mixed powder into shape on a press with a pressure of 400-600MPa and a holding time of 1-5min. S4. Sintering: The green blanks are placed in a vacuum furnace for sintering, heated to 900-1000°C at a heating rate of 5-10°C per minute, held for 30-90 minutes, and finally cooled to room temperature with the furnace.

[0009] Compared with the prior art, the present invention has the following beneficial effects:

[0010] 1. The raw materials of this invention are readily available, the cost is low, the process is simple, and the parameters are easy to control, so it can be used on a large scale for the production of sliding bearings.

[0011] 2. The high-strength self-lubricating bearing material of the present invention has a low relative sintering density, high yield strength, and good wear resistance, and is therefore widely used in mechanical equipment such as steel, metallurgy, and agricultural machinery. It is especially suitable for occasions where lubrication cannot be added during service. Attached Figure Description

[0012] Figure 1 This is a microstructure of the alloy without the addition of MoS2.

[0013] Figure 2 Microstructure of the alloy with 4% MoS2 by weight.

[0014] Figure 3 Microstructure of the alloy with 6% MoS2 by weight.

[0015] Figure 4 Microstructure of the alloy with 8% MoS2 by weight. Implementation

[0016] The present invention will be further described in detail below with reference to the embodiments. Example 1

[0017] In this embodiment, the weight percentage of the raw materials is: 10% aluminum powder, 4% nickel powder, 6% copper-clad iron powder, and the remainder is copper powder.

[0018] Step 1: Measure aluminum powder, nickel powder, copper-clad iron powder, and copper powder using an electronic balance, and place them in a grinding mill for uniform mixing for 1-6 hours.

[0019] Step 2: Press the mixed powder into shape at a pressure of 400-600 MPa for 1-5 minutes.

[0020] Step 3: The green embryo is placed in a vacuum furnace for sintering, heated to 900-1000℃ at a rate of 5-10℃ / min, held for 30-90min, and finally cooled to room temperature in the furnace to obtain the sample. The microstructure of the sample is as follows: Figure 1 As shown. Example 2

[0021] In this embodiment, the weight percentage of the raw materials is: 10% aluminum powder, 4% nickel powder, 6% copper-clad iron powder, 4% MoS2 powder, and the remainder is copper powder.

[0022] Step 1: Measure aluminum powder, nickel powder, copper-clad iron powder, MoS2, and copper powder using an electronic balance, and place them in a grinding mill for uniform mixing for 1-6 hours.

[0023] Step 2: Press the mixed powder into shape at a pressure of 400-600 MPa for 1-5 minutes.

[0024] Step 3: The green embryo is placed in a vacuum furnace for sintering, heated to 900-1000℃ at a rate of 5-10℃ / min, held for 30-90min, and finally cooled to room temperature in the furnace to obtain the sample. The microstructure of the sample is as follows: Figure 2 As shown. Example 3

[0025] In this embodiment, the weight percentage of the raw materials is: 10% aluminum powder, 4% nickel powder, 6% copper-clad iron powder, 6% MoS2 powder, and the remainder is copper powder.

[0026] Step 1: Measure aluminum powder, nickel powder, copper-clad iron powder, MoS2, and copper powder using an electronic balance, and place them in a grinding mill for uniform mixing for 1-6 hours.

[0027] Step 2: Press the mixed powder into shape at a pressure of 400-600 MPa for 1-5 minutes.

[0028] Step 3: The green embryo is placed in a vacuum furnace for sintering, heated to 900-1000℃ at a rate of 5-10℃ / min, held for 30-90min, and finally cooled to room temperature in the furnace to obtain the sample. The microstructure of the sample is as follows: Figure 3 As shown. Example 4

[0029] In this embodiment, the weight percentage of the raw materials is: 10% aluminum powder, 4% nickel powder, 6% copper-clad iron powder, 8% MoS2 powder, and the remainder is copper powder.

[0030] Step 1: Measure aluminum powder, nickel powder, copper-clad iron powder, MoS2, and copper powder using an electronic balance, and place them in a grinding mill for uniform mixing for 1-6 hours.

[0031] Step 2: Press the mixed powder into shape at a pressure of 400-600 MPa for 1-5 minutes.

[0032] Step 3: The green embryo is placed in a vacuum furnace for sintering, heated to 900-1000℃ at a rate of 5-10℃ / min, held for 30-90min, and finally cooled to room temperature in the furnace to obtain the sample. The microstructure of the sample is as follows: Figure 4 As shown.

[0033] The sintering density, hardness, and yield strength of the materials obtained in Examples 1-4 were measured, and the wear results are shown in Table 1 below: <![CDATA[MoS2 content (weight ratio)]]> Sintered density (%) Hardness (HB) Yield strength (MPa) Wear amount (mg) Example 1 0% 85-90 105-110 300-320 5-6 Example 2 4% 85-90 115-120 360-390 5-6 Example 3 6% 80-85 115-120 350-380 5-6 Example 4 8% 80-85 110-115 350-370 6-11 Based on the above measurement results and the alloy microstructure, it can be seen that: (1) The prepared material has a uniform structure and uniform pores, such as Figures 1-4 As shown.

[0034] (2) During the sintering process, the addition of molybdenum disulfide hinders diffusion and the formation of sintering necks. At high temperatures, molybdenum disulfide decomposes and reacts to form new sulfides, creating pores in the original locations of the molybdenum disulfide. Therefore, the prepared bearing material has high porosity and a relative sintering density of 80-90%, which allows the bearing to store more lubricating oil before use. Compared to materials without molybdenum disulfide, it has more pores, such as... Figures 1-4 As shown in Table 1, the porosity is also greatly improved.

[0035] (3) The decomposition of molybdenum disulfide and its reaction with iron and copper to form sulfides strengthen the material. Therefore, the yield strength of the prepared bearing material reaches more than 350 MPa, which is nearly 100 MPa higher than that of the material without molybdenum disulfide (Example 1). The hardness is 110-120 HB, which is 10-15 HB higher than that of the material without molybdenum disulfide (Example 1). The wear resistance is good. The friction sample is in the shape of a small round pin. The grinding material is 40Cr steel. The rotation speed is 150 rpm, the pressure is 20 N, and the test time is 30 minutes. The wear amount of the material with molybdenum disulfide is 5-11 mg, which is similar to that of the material without molybdenum disulfide.

[0036] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A high-strength self-lubricating bearing material, characterized in that, The raw materials include the following weight percentages: 8%–11% aluminum powder, 3%–5% nickel powder, 5%–10% copper-clad iron powder, 4%–8% MoS2 powder, and the balance is copper powder. The high-strength self-lubricating bearing material is made by sintering the constituent raw materials. During the sintering process, at a sintering temperature of 900-1000℃, the MoS2 powder decomposes and becomes pores in its original position. The decomposed MoS2 reacts with the iron and copper in the copper-coated iron powder to generate sulfides. The relative sintering density of the high-strength self-lubricating bearing material is 80%-90%, and the yield strength is ≥350MPa.

2. The high-strength self-lubricating bearing material as described in claim 1, characterized in that, The MoS2 powder has a weight percentage of 6%.

3. The high-strength self-lubricating bearing material as described in claim 1, characterized in that, The aluminum powder has a weight percentage of 10%, the nickel powder has a weight percentage of 4%, and the copper-clad iron powder has a weight percentage of 6%.

4. A method for preparing a high-strength self-lubricating bearing material, used to prepare the high-strength self-lubricating bearing material as described in any one of claims 1-3, characterized in that, Includes the following steps: S1. First, obtain the raw materials according to the following weight percentages: 8% to 11% aluminum powder, 3% to 5% nickel powder, 5% to 10% copper-clad iron powder, 4% to 8% MoS2 powder, and the remainder is copper powder. S2. Mixing: Put the raw materials obtained in step S1 into a grinding mill and mix for 1 to 6 hours; S3. Pressing: Press the mixed powder into shape on a press with a pressure of 400-600MPa and a holding time of 1-5min. S4. Sintering: The green blanks are placed in a vacuum furnace for sintering, heated to 900-1000°C at a heating rate of 5-10°C per minute, held for 30-90 minutes, and finally cooled to room temperature with the furnace.

Citation Information

Patent Citations

  • Car synchronous ring material and preparing method

    CN108480645A