A nitrogen / sulfur-doped nickel-iron layered hydroxide oxygen evolution composite catalytic material, a preparation method therefor, and an application thereof

By growing nitrogen/sulfur-doped nickel-iron layered hydroxides in situ on a conductive substrate, the problems of poor conductivity and complicated synthesis were solved, and a highly active electrocatalytic material suitable for the oxygen evolution reaction of water electrolysis was prepared.

CN117926328BActive Publication Date: 2026-11-24HANGZHOU NORMAL UNIVERSITY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410036508.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-10
Publication Date
2026-11-24
Estimated Expiration
2044-01-10

AI Technical Summary

Technical Problem

Existing commercial catalysts such as ruthenium oxide and iridium oxide are expensive, and transition metal hydroxides such as iron-nickel layered bimetallic hydroxides have poor conductivity and complicated synthesis processes, which limit their application in hydrogen production by water electrolysis.

Method used

A one-step hydrothermal method was used to grow nitrogen/sulfur-doped nickel-iron layered hydroxides in situ on a conductive substrate. By controlling the morphology and doping amount, the conductivity and activity of the composite catalytic material with a petal-like structure were improved.

Benefits of technology

It achieves low-cost, high-activity electrochemical catalytic performance, overcomes the limitations of active sites, enhances the specific surface area and electron transport rate of the material, and is suitable for the oxygen evolution reaction in water electrolysis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117926328B_ABST
    Figure CN117926328B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a nitrogen / sulfur-doped nickel-iron layered hydroxide oxygen evolution reaction (OER) composite catalyst. The method includes: dissolving a nitrogen / sulfur source, a nickel source, an iron source, urea, and ammonium fluoride in water to form a precursor solution; completely immersing a conductive substrate in the precursor solution and then performing a hydrothermal reaction to obtain nitrogen / sulfur-doped nickel-iron layered hydroxide. This invention also discloses the nitrogen / sulfur-doped nickel-iron layered hydroxide OER composite catalyst obtained by the above preparation method and its application in the oxygen evolution reaction of water electrolysis. The preparation method provided by this invention incorporates nitrogen / sulfur into nickel-iron layered hydroxide in one step and grows it in situ on the surface of a conductive substrate, exhibiting excellent electrochemical catalytic performance in the oxygen evolution reaction of water electrolysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the fields of nanomaterials technology and electrochemical energy conversion, specifically relating to a nitrogen / sulfur-doped nickel-iron layered hydroxide oxygen evolution composite catalytic material, its preparation method, and its application. Background Technology

[0002] Hydrogen energy has a high calorific value (1.4 × 10⁻⁶). 8 With advantages such as high efficiency (J / Kg), its fuel reaction products are water and oxygen, with no carbon emissions, making it an ideal clean energy source to replace fossil fuels. Compared to other hydrogen production technologies, water electrolysis hydrogen production technology has zero carbon emissions throughout the entire process, making it a highly promising hydrogen production technology.

[0003] The oxygen evolution reaction (OER) is a crucial step in the water electrolysis process for hydrogen production. This is because, compared to the hydrogen evolution reaction (HER), the OER is a typical four-electron reaction with a more complex reaction pathway and slower kinetics. Currently, commercial catalysts ruthenium oxide and iridium oxide exhibit excellent OER activity, but their high price hinders their large-scale application. Therefore, developing low-cost, high-activity OER anode catalysts is of great significance.

[0004] Hydroxides of transition metal elements (such as iron, nickel, cobalt, and manganese) are promising catalytic materials for water electrolysis due to their excellent two-dimensional layered structure and tunable chemical composition. However, as hydroxides, they exhibit poor conductivity and limited active sites, requiring rational material design to improve their conductivity and activity. Chinese Patent CN110152673A discloses an iron-nickel layered bimetallic hydroxide / nickel foam composite material, its preparation method, and its application. The iron-nickel layered bimetallic hydroxide / nickel foam composite material is prepared using a two-step hydrothermal method, but its conductivity and activity are limited at 100 mA·cm⁻¹. -2 At the current density, the overpotential for oxygen evolution is still much greater than 300mV. Chinese patent CN113026045A discloses a method for preparing nickel foam-supported Ni(OH)2 / FeOOH nanoflower materials. The steps involve first obtaining a nickel-iron layered double hydroxide nanoarray through a hydrothermal reaction, and then modifying the generated nickel-iron layered hydroxide with sodium sulfide or thiourea. The preparation steps are cumbersome.

[0005] Therefore, developing a nickel-iron layered hydroxide catalytic material with a simple preparation process and high activity is of great significance for its industrial application. Summary of the Invention

[0006] The purpose of this invention is to provide a method for preparing a nitrogen / sulfur-doped nickel-iron layered hydroxide oxygen evolution composite catalytic material, as well as the prepared composite catalytic material and its application in the oxygen evolution reaction of water electrolysis. The preparation method provided by this invention involves one-step doping of nitrogen / sulfur into nickel-iron layered hydroxide and in-situ growth on the surface of a conductive substrate, resulting in excellent electrochemical catalytic performance in the oxygen evolution reaction of water electrolysis.

[0007] This invention provides the following technical solution:

[0008] The first aspect of the present invention provides a method for preparing a nitrogen / sulfur-doped nickel-iron layered hydroxide oxygen evolution composite catalyst material. The preparation method includes: dissolving a nitrogen / sulfur source, a nickel source, an iron source, urea and ammonium fluoride in water to form a precursor solution; completely immersing a conductive substrate in the precursor solution and then performing a hydrothermal reaction to obtain a nitrogen / sulfur-doped nickel-iron layered hydroxide.

[0009] This invention employs a simple one-step hydrothermal method to achieve in-situ growth, morphology control, and direct nitrogen / sulfur doping of nickel-iron layered hydroxides on conductive substrates, enriching the synthesis and preparation technology of nickel-iron layered hydroxides. At the same time, the simple preparation process greatly expands its commercial application value.

[0010] The nitrogen / sulfur source in the precursor solution is ammonium sulfate, the nickel source is nickel nitrate hexahydrate or nickel chloride, and the iron source is ferric nitrate nonahydrate or ferric chloride.

[0011] The nitrogen / sulfur source in the precursor solution has a concentration of 0.005 mol / L to 0.05 mol / L, the nickel source has a concentration of 0.03 mol / L to 0.045 mol / L, the iron source has a concentration of 0.005 mol / L to 0.175 mol / L, the urea has a concentration of 0.2 mol / L to 0.4 mol / L, and the ammonium fluoride has a concentration of 0.05 mol / L to 0.175 mol / L.

[0012] The hydrothermal reaction is carried out at a temperature of 100–160°C for 8–16 hours.

[0013] This invention regulates the morphology of nickel-iron layered hydroxides and the amount of nitrogen / sulfur doping by adjusting the concentration of the precursor solution and the conditions of the hydrothermal reaction, thereby further regulating the electrochemical performance of the composite catalytic material.

[0014] Preferably, the concentration of ammonium sulfate in the precursor solution is 0.005 mol / L to 0.02 mol / L; the hydrothermal reaction temperature is 120 to 150 °C. Within the above process range, a more uniform petal-like morphology can be obtained, and a suitable nitrogen / sulfur doping amount can be achieved, which is beneficial to improving the electrochemical performance of the composite catalytic material.

[0015] More preferably, the concentration of the ammonium sulfate is 0.005 mol / L to 0.01 mol / L.

[0016] Preferably, the conductive substrate is selected from nickel foam, nickel-iron foam, copper foam, carbon paper, or graphite.

[0017] More preferably, the conductive substrate is selected from nickel foam.

[0018] Preferably, the preparation method further includes: after hydrothermal reaction, cooling and removing the conductive substrate, washing and drying to obtain nitrogen-doped nickel-iron layered hydroxide nanosheets. The drying temperature (drying after hydrothermal reaction and cleaning) is 40–60°C, the time is 6–12 hours, and drying is performed in a constant temperature drying oven.

[0019] A second aspect of the present invention provides a nitrogen / sulfur-doped nickel-iron layered hydroxide oxygen evolution composite catalyst obtained according to the above preparation method.

[0020] The nitrogen / sulfur-doped nickel-iron layered hydroxide nanosheets are grown in situ on a conductive substrate and interconnected to form a petal-like structure.

[0021] The nitrogen / sulfur-doped nickel-iron layered hydroxide composite catalytic material provided by this invention optimizes the electronic structure of nickel-iron layered hydroxide with nitrogen / sulfur doping, increases the specific surface area of ​​active sites with petal-like morphology, improves the conductivity of the material with composite material structure, and accelerates the ion and charge transport rate. When used as an electrode material, it exhibits excellent electrochemical performance.

[0022] The third aspect of this invention provides an application of the above-mentioned nitrogen / sulfur-doped nickel-iron layered hydroxide oxygen evolution composite catalyst as a catalyst for water electrolysis; further, its application as an anode material in the oxygen evolution reaction of water electrolysis under alkaline conditions.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] This invention provides a method for preparing a highly active nitrogen / sulfur one-step doped nickel-iron layered hydroxide composite catalyst material grown in situ on a conductive substrate. This method solves the problems of poor conductivity and cumbersome synthesis control processes associated with transition metal hydroxides. It also enables the adjustment of the local electronic configuration of transition metal hydroxides to improve their intrinsic activity in the oxygen evolution reaction, thus overcoming the limitation of transition metal hydroxide activity. Therefore, the preparation method provided by this invention greatly expands the commercial application value of nickel-iron layered hydroxides.

[0025] The composite catalytic material provided by this invention modulates the local electronic structure of transition metal hydroxides through nitrogen / sulfur doping, accelerating their electron transfer rate and lowering their reaction energy barrier, thereby overcoming the limited active sites and enhancing their intrinsic activity. Nitrogen / sulfur-doped nickel-iron layered hydroxide nanosheets are constructed into a petal-like morphology and grown on the surface of a conductive substrate, increasing the specific surface area of ​​the material and the number of exposed active sites. Utilizing the conductive substrate as a self-supporting material, the nickel-iron layered hydroxide, as the active substance, is grown on its surface, greatly avoiding problems such as poor contact between the catalytic material and the electrode surface, poor conductivity, and adhesion of interfacial gas products. Therefore, the composite catalytic material provided by this invention possesses excellent electrochemical catalytic performance and is expected to replace precious metal electrode materials. It is a novel electrochemical catalytic material that meets the needs of new energy sources and can be used as a novel electrocatalytic oxygen evolution anode catalytic material, promoting its industrial application in water electrolysis. Attached Figure Description

[0026] Figure 1 This is a scanning electron microscope image of the nitrogen / sulfur-doped nickel-iron layered hydroxide composite catalytic material prepared in Example 1.

[0027] Figure 2 This is an energy dispersive X-ray spectral surface scan of the nitrogen / sulfur-doped nickel-iron layered hydroxide composite catalytic material prepared in Example 1.

[0028] Figure 3 This is the X-ray photoelectron spectrum of the nitrogen / sulfur-doped nickel-iron layered hydroxide composite catalytic material prepared in Example 1.

[0029] Figure 4 The figures show linear sweep voltammetry results of the nitrogen / sulfur doped nickel-iron layered hydroxide composite catalytic materials prepared in Examples 1-4, the nickel-iron layered hydroxide nanosheet catalytic material prepared in Comparative Example 1, and the pure nickel foam material in Comparative Example 2. Detailed Implementation

[0030] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments.

[0031] Unless otherwise specified, conventional reagents and general methods in this field may be used in the following description.

[0032] A method for preparing a nitrogen / sulfur-doped nickel-iron layered hydroxide oxygen evolution composite catalyst material includes the following steps:

[0033] 1.1) Add nickel source, iron source, nitrogen / sulfur source, urea and ammonium fluoride to deionized water and stir;

[0034] 1.2) Transfer the above solution and the pretreated nickel foam substrate to a reactor and place it in an oven for hydrothermal reaction;

[0035] 1.3) After cooling, remove the nickel foam, wash it, and dry it in an oven to finally obtain the desired composite catalyst material.

[0036] Specifically:

[0037] In 1.1), the added iron source concentration is 0.005 mol / L to 0.175 mol / L, the nickel source concentration is 0.03 mol / L to 0.045 mol / L, the nitrogen / sulfur source concentration is 0.005 mol / L to 0.05 mol / L, the urea concentration is 0.2 mol / L to 0.4 mol / L, and the ammonium fluoride concentration is 0.05 mol / L to 0.175 mol / L.

[0038] In 1.2), the temperature of the hydrothermal reaction is 100–160℃, and the reaction time is 8–16h.

[0039] In step 1.3), the obtained hydrothermal reaction-induced nickel foam is placed in a constant temperature drying oven for drying at a temperature of 40–60°C for 8–16 hours.

[0040] The above preparation method employs a hydrothermal synthesis approach to synthesize nitrogen / sulfur-doped nickel-iron layered hydroxide nanosheet catalytic materials in a single step. The preparation process is simple, the raw material cost is low, and the reaction conditions are easily controlled. The prepared catalytic material exhibits high catalytic activity and a lower overpotential. The preparation method provided by this invention can be applied on a large scale in industrial production and has good practicality.

[0041] In some embodiments of the preparation method provided by this invention, the nickel foam is not particularly limited, as long as it meets the purpose of this application. The nickel foam can also be 1cm × 2cm in size.

[0042] In some embodiments of the preparation method provided by the present invention, preferably, the nickel foam is pretreated, specifically including the following steps: first, the nickel foam is cut into sheets of 1cm×3cm size, placed in a 1mol / L hydrochloric acid solution for ultrasonic cleaning for about 15min, then acetone, deionized water and anhydrous ethanol are used in sequence for ultrasonic cleaning for about 15min each to remove surface oil and oxides, and finally placed in a vacuum oven for drying to obtain clean nickel foam sheets.

[0043] The present invention will be further described in detail below with reference to specific embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0044] Example 1

[0045] Nickel nitrate hexahydrate, ferric nitrate nonahydrate, ammonium sulfate, urea, and ammonium fluoride were dissolved in 20 mL of deionized water and stirred for 30 min until a clear, homogeneous solution was formed. The concentrations of nickel nitrate hexahydrate, ferric nitrate nonahydrate, ammonium sulfate, urea, and ammonium fluoride were 0.0375 mol / L, 0.0085 mol / L, 0.01 mol / L, 0.2997 mol / L, and 0.1202 mol / L, respectively. The solution and pretreated nickel foam were transferred to a 50 mL polytetrafluoroethylene (PTFE) stainless steel high-pressure reactor, sealed, and reacted in an oven at 120 °C for 12 h. After the reactor cooled to room temperature, the nickel foam was removed, washed with deionized water, and dried in an oven to obtain a nitrogen / sulfur-doped nickel-iron layered hydroxide composite catalyst.

[0046] Example 2

[0047] Nickel nitrate hexahydrate, ferric nitrate nonahydrate, ammonium sulfate, urea, and ammonium fluoride were dissolved in 20 mL of deionized water and stirred for 30 min until a clear, homogeneous solution was formed. The concentrations of nickel nitrate hexahydrate, ferric nitrate nonahydrate, ammonium sulfate, urea, and ammonium fluoride were 0.0375 mol / L, 0.0085 mol / L, 0.01 mol / L, 0.2997 mol / L, and 0.1202 mol / L, respectively. The solution and pretreated nickel foam were transferred to a 50 mL polytetrafluoroethylene (PTFE) stainless steel high-pressure reactor, sealed, and reacted in an oven at 150 °C for 12 h. After the reactor cooled to room temperature, the nickel foam was removed, washed with deionized water, and dried in an oven to obtain a nitrogen / sulfur-doped nickel-iron layered hydroxide composite catalyst.

[0048] Example 3

[0049] Nickel nitrate hexahydrate, ferric nitrate nonahydrate, ammonium sulfate, urea, and ammonium fluoride were dissolved in 20 mL of deionized water and stirred for 30 min until a transparent and homogeneous solution was formed. The concentrations of nickel nitrate hexahydrate, ferric nitrate nonahydrate, ammonium sulfate, urea, and ammonium fluoride were 0.0375 mol / L, 0.0085 mol / L, 0.005 mol / L, 0.2997 mol / L, and 0.1202 mol / L, respectively. The solution and pretreated nickel foam were transferred to a 50 mL polytetrafluoroethylene (PTFE) stainless steel high-pressure reactor, sealed, and reacted in an oven at 120 °C for 12 h. After the reactor cooled to room temperature, the nickel foam was removed, washed with deionized water, and dried in an oven to obtain a nitrogen / sulfur-doped nickel-iron layered hydroxide composite catalyst.

[0050] Example 4

[0051] Nickel nitrate hexahydrate, ferric nitrate nonahydrate, ammonium sulfate, urea, and ammonium fluoride were dissolved in 20 mL of deionized water and stirred for 30 min until a transparent and homogeneous solution was formed. The concentrations of nickel nitrate hexahydrate, ferric nitrate nonahydrate, ammonium sulfate, urea, and ammonium fluoride were 0.0375 mol / L, 0.0085 mol / L, 0.02 mol / L, 0.2997 mol / L, and 0.1202 mol / L, respectively. The solution and pretreated nickel foam were transferred to a 50 mL polytetrafluoroethylene (PTFE) stainless steel high-pressure reactor, sealed, and reacted in an oven at 120 °C for 12 h. After the reactor cooled to room temperature, the nickel foam was removed, washed with deionized water, and dried in an oven to obtain a nitrogen / sulfur-doped nickel-iron layered hydroxide composite catalyst.

[0052] Comparative Example 1

[0053] Nickel nitrate hexahydrate, ferric nitrate nonahydrate, urea, and ammonium fluoride were dissolved in 20 mL of deionized water and stirred for 30 min until a transparent, homogeneous solution was formed. The concentrations of nickel nitrate hexahydrate, ferric nitrate nonahydrate, urea, and ammonium fluoride were 0.0375 mol / L, 0.0085 mol / L, 0.2997 mol / L, and 0.1202 mol / L, respectively. The solution and the pretreated nickel foam were transferred to a 50 mL polytetrafluoroethylene (PTFE) stainless steel high-pressure reactor, sealed, and reacted in an oven at 120 °C for 12 h. After the reactor cooled to room temperature, the nickel foam was removed, washed with deionized water, and dried in an oven to obtain the nickel-iron layered hydroxide nanosheet catalyst material.

[0054] Comparative Example 2

[0055] Pretreatment of nickel foam: Nickel foam was cut into 1cm × 3cm sheets and ultrasonically cleaned in a 1mol / L dilute hydrochloric acid solution for about 15 minutes. Then, it was ultrasonically cleaned sequentially with acetone, deionized water, and anhydrous ethanol for about 15 minutes each to remove oil and oxides from the surface of the nickel foam. Finally, it was dried in a vacuum drying oven to obtain the cleaned nickel foam substrate material. No further treatment is required, and electrochemical performance testing can be performed directly.

[0056] Application Example 1

[0057] The oxygen evolution performance of the catalytic material was evaluated using linear sweep voltammetry at a scan rate of 5 mV / s. -1 The specific electrochemical tests were conducted using a three-electrode system at room temperature, with the prepared catalytic material as the working electrode, the Ag|AgCl electrode as the reference electrode, and the stone rod electrode as the counter electrode. The electrolyte was a 1 mol / L KOH solution (pH = 13.8).

[0058] Material morphology and structure analysis:

[0059] Figure 1 This is a scanning electron microscope image of nitrogen / sulfur-doped nickel-iron layered hydroxide nanosheets from Example 1. Figure 1 The layered nanosheets shown in (a) are interconnected to form a petal-like structure. The petal-like nanosheets are uniform in size and distributed in a staggered manner, which is conducive to shortening the distance of electron transport. The nanochannels and suitable mesoporous structures provided promote ion transport. Figure 1 As shown in (b), the petal-shaped nanosheets constructed thereon grow in situ on the surface of nickel foam, which increases the specific surface area of ​​the material and exposes more active sites, thereby greatly improving the catalytic activity.

[0060] Figure 2 and Figure 3 The images show the energy dispersive X-ray spectral surface scan and X-ray photoelectron spectroscopy of the nitrogen / sulfur-doped nickel-iron layered hydroxide nanosheets from Example 1, respectively. The images show the presence of Ni, Fe, O, N, and S, confirming the successful introduction of N and S.

[0061] Oxygen evolution performance testing and analysis:

[0062] Figure 4 Linear voltammetric scans of the nitrogen / sulfur-doped nickel-iron layered hydroxide composite catalytic materials of Examples 1-4, the nickel-iron layered hydroxide nanosheet catalytic material of Comparative Example 1, and the nickel foam substrate material of Comparative Example 2 are shown below. Figure 4 As shown, the nitrogen / sulfur-doped nickel-iron layered hydroxide composite catalytic material exhibits a significantly reduced overpotential compared to nickel-iron layered hydroxide nanosheet catalytic materials and nickel foam substrate materials, demonstrating excellent electrocatalytic oxygen evolution performance.

[0063] In summary, the nitrogen / sulfur-doped nickel-iron layered hydroxide composite catalytic material of the present invention is inexpensive, easy to prepare, and has high electrocatalytic oxygen evolution activity, and can be used as an electrocatalytic oxygen evolution anode material in the field of water electrolysis.

[0064] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.

Claims

1. A method for preparing a nitrogen / sulfur-doped nickel-iron layered hydroxide oxygen evolution composite catalyst, characterized in that, The preparation method includes: dissolving a nitrogen / sulfur source, a nickel source, an iron source, urea, and ammonium fluoride in water to form a precursor solution; completely immersing a conductive substrate in the precursor solution and then performing a hydrothermal reaction to obtain a nitrogen / sulfur-doped nickel-iron layered hydroxide; wherein the nitrogen / sulfur source is ammonium sulfate, the nickel source is nickel nitrate hexahydrate or nickel chloride, and the iron source is ferric nitrate nonahydrate or ferric chloride.

2. The preparation method of the nitrogen / sulfur-doped nickel-iron layered hydroxide oxygen evolution composite catalyst according to claim 1, characterized in that, The nitrogen / sulfur source in the precursor solution has a concentration of 0.005 mol / L to 0.05 mol / L, the nickel source has a concentration of 0.03 mol / L to 0.045 mol / L, the iron source has a concentration of 0.005 mol / L to 0.175 mol / L, the urea has a concentration of 0.2 mol / L to 0.4 mol / L, and the ammonium fluoride has a concentration of 0.05 mol / L to 0.175 mol / L.

3. The preparation method of the nitrogen / sulfur-doped nickel-iron layered hydroxide oxygen evolution composite catalyst according to claim 2, characterized in that, The hydrothermal reaction is carried out at a temperature of 100~160℃ for 8~16 hours.

4. The preparation method of the nitrogen / sulfur-doped nickel-iron layered hydroxide oxygen evolution composite catalyst according to claim 2, characterized in that, The concentration of ammonium sulfate in the precursor solution is 0.005 mol / L to 0.02 mol / L; the temperature of the hydrothermal reaction is 120 to 150℃.

5. The preparation method of the nitrogen / sulfur-doped nickel-iron layered hydroxide oxygen evolution composite catalyst according to claim 1, characterized in that, The conductive substrate is selected from nickel foam, nickel-iron foam, copper foam, carbon paper, or graphite.

6. A nitrogen / sulfur-doped nickel-iron layered hydroxide oxygen evolution composite catalyst material obtained by the preparation method according to any one of claims 1-5.

7. The nitrogen / sulfur-doped nickel-iron layered hydroxide oxygen evolution composite catalyst according to claim 6, characterized in that, In the composite catalytic material, nitrogen / sulfur-doped nickel-iron layered hydroxide nanosheets are grown in situ on a conductive substrate and interconnected to form a petal-like structure.

8. The application of the nitrogen / sulfur-doped nickel-iron layered hydroxide oxygen evolution composite catalyst of claim 6 in the oxygen evolution reaction of water electrolysis.

Citation Information

Patent Citations

  • Iron-nickel layered double metal hydroxide / foam nickel composite material and preparation method and application thereof

    CN110152673A

  • Preparation method of foamed nickel loaded Ni(OH)2 / FeOOH nanoflower material

    CN113026045A

  • Sulfur-doped ferronickel-based composite electrocatalyst and preparation method and application thereof

    CN115584534A

  • Preparation method of sulfur-doped nickel-iron hydroxide ultrathin nanosheet

    CN116282230A