LED chip and preparation method thereof

By combining primary and secondary etching processes, the problem of photoresist overexposure in the TCL photolithography process for high-voltage LED chips was solved, enabling precise distance control between MESA and TCL, and improving luminous efficiency and production efficiency.

CN117936662BActive Publication Date: 2026-11-20JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410116386.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-29
Publication Date
2026-11-20
Estimated Expiration
2044-01-29

AI Technical Summary

Technical Problem

During the photolithography process of high-voltage LED chips in TCL, the ISO isolation trenches are relatively deep, which requires a large amount of exposure. This leads to overexposure of the photoresist in non-trench areas, resulting in a significant difference between the actual linewidth and the designed linewidth, wasting the light-emitting area. Furthermore, the actual distance between MESA and TCL is inaccurate, affecting the luminous efficiency.

Method used

A combination of primary and secondary etching processes is adopted, and the actual distance between MESA and TCL is controlled by wet and dry etching techniques to ensure that the spacing between MESA and TCL is 3μm to 5μm, thereby reducing the overexposure of photoresist and improving the utilization rate of light-emitting area.

Benefits of technology

By effectively controlling the actual distance between MESA and TCL, the light-emitting area is increased, the luminous efficacy of the LED chip is improved, and the manufacturing steps are reduced, thus increasing production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117936662B_ABST
    Figure CN117936662B_ABST
Patent Text Reader

Abstract

The application provides an LED chip and a preparation method thereof. The method comprises the following steps: providing a semi-finished LED chip, the semi-finished LED chip comprising a PSS substrate, a gallium nitride epitaxial layer and a current blocking layer deposited on the PSS substrate in sequence; manufacturing a TCL film layer on the gallium nitride epitaxial layer and the current blocking layer, and forming a MESA / TCL photoetching pattern through a photoetching technology; etching the TCL selectively through a first etching, and then etching through a second etching to expose an N-type semiconductor layer of the gallium nitride epitaxial layer; manufacturing P / N electrodes for electrically connecting with a P-type semiconductor layer and the N-type semiconductor layer of the gallium nitride epitaxial layer respectively; and manufacturing a protective layer, a part of the electrode is exposed for packaging a solder wire, and the rest of the electrode is completely covered. Specifically, the photoetching of the two processes of MESA and TCL is combined into one process, the distance between the two can be better controlled, the light emitting area is greatly increased, and the light efficiency of the chip is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor technology, and in particular to an LED chip and its fabrication method. Background Technology

[0002] Because the ISO isolation trenches of high-voltage LED chips are deep, a larger exposure is required during TCL photolithography to ensure that the photoresist in the trenches is developed cleanly. However, a larger exposure will cause the photoresist in the non-trench areas to be overexposed, resulting in a significant difference between the actual linewidth and the designed linewidth. This causes the TCL to be further away from MESA, wasting a portion of the light-emitting area.

[0003] Specifically, the conventional process for manufacturing high-voltage LEDs is as follows: 1. MESA (Metal-on-Semiconductor Alignment), removing part of the P-type semiconductor and light-emitting layer to expose the N-type semiconductor; 2. ISO (Isolation Layer), fabricating the isolation trench; 3. CBL (Current Block Layer), fabricating the current blocking layer; 4. TCL (Transparent Conductive Layer), fabricating the transparent conductive layer; 5. PAD (Electrical Anode), evaporating the electrode; 6. PSV (Power Seal Layer), fabricating the protective layer. MESA and TCL are two separate photolithography steps, designed with a 3μm to 7μm gap between them to ensure a safe distance and prevent chip leakage, short circuits, or other failures. However, due to the high-voltage ISO trench, a larger exposure is required, causing overexposure of the photoresist in non-trench areas. This results in an actual linewidth difference of 2μm to 5μm from the designed linewidth, leading to a final actual distance of 5μm to 12μm between MESA and TCL. Summary of the Invention

[0004] Based on this, the purpose of this invention is to provide an LED chip and its fabrication method, which aims to control the actual distance between MESA and TCL, and avoid wasting the light-emitting area during the manufacturing process, so as to prevent the luminous efficiency from not reaching the optimal level.

[0005] According to an embodiment of the present invention, an LED chip fabrication method includes:

[0006] A semi-finished LED chip is provided, the semi-finished LED chip comprising a PSS substrate, and a gallium nitride epitaxial stack and a current blocking layer sequentially deposited on the PSS substrate;

[0007] A TCL film layer was fabricated on the gallium nitride epitaxial stack and the current blocking layer, and a MESA / TCL photolithographic pattern was formed by photolithography.

[0008] TCL is selectively etched using wet etching, followed by dry etching, to expose the N-type semiconductor layer of the gallium nitride epitaxial stack.

[0009] P / N electrodes are fabricated for electrical connection to the P-type and N-type semiconductor layers of a gallium nitride epitaxial stack, respectively.

[0010] A protective layer is prepared, with some electrodes exposed to encapsulate the bonding wires, while the rest are completely covered.

[0011] Furthermore, the step of providing a semi-finished LED chip, the semi-finished LED chip comprising a PSS substrate, and a gallium nitride epitaxial layer and a current blocking layer sequentially deposited on the PSS substrate, includes:

[0012] A wafer substrate is provided, and PSS fabrication is performed to obtain a PSS substrate;

[0013] Gallium nitride epitaxial stacks are fabricated on PSS substrates, wherein the gallium nitride epitaxial stacks include a buffer layer, an N-type semiconductor layer, a light-emitting layer, and a P-type semiconductor layer sequentially deposited on the PSS substrates.

[0014] The isolation trench region pattern is formed on the gallium nitride epitaxial stack using photolithography, and the gallium nitride epitaxial stack is etched until part of the PSS substrate is exposed.

[0015] The current blocking layer is fabricated in the region of the P-type semiconductor layer to reduce the recombination of charge carriers directly below the metal electrode and to prevent the radiated photons from being absorbed and blocked by the metal.

[0016] Furthermore, in the step of selectively etching the TCL through a first etching and then exposing the N-type semiconductor layer of the gallium nitride epitaxial stack through a second etching, the actual distance between MESA and TCL is 3μm to 5μm.

[0017] Furthermore, in the step of selectively etching the TCL through a first etching and then exposing the N-type semiconductor layer of the gallium nitride epitaxial stack through a second etching, the actual etched TCL has a spacing of 0μm to 1μm compared with the TCL design pattern.

[0018] Furthermore, in the step of selectively etching the TCL through a first etching and then exposing the N-type semiconductor layer of the gallium nitride epitaxial stack through a second etching, the actual etched MESA has a spacing of 1μm to 3μm compared with the MESA design pattern.

[0019] Furthermore, the material of the current blocking layer is SiO2, and the thickness of the current blocking layer is 150nm to 420nm.

[0020] Furthermore, the material of the TCL film is either indium tin oxide or indium zinc oxide, and the thickness of the TCL film is 25nm to 150nm.

[0021] Furthermore, the first etching is a wet etching process, and the second etching is a dry etching process.

[0022] An LED chip according to an embodiment of the present invention is prepared according to the above-described LED chip preparation method.

[0023] Furthermore, the actual distance between MESA and TCL is 3μm to 5μm.

[0024] This invention provides an LED chip and its fabrication method. The method includes providing a semi-finished LED chip, which includes a PSS substrate and a gallium nitride epitaxial layer and a current blocking layer sequentially deposited on the PSS substrate; fabricating a TCL film layer on the gallium nitride epitaxial layer and the current blocking layer, and forming a MESA / TCL photolithographic pattern using photolithography; selectively etching the TCL layer through a first etching step, followed by a second etching step to expose the N-type semiconductor layer of the gallium nitride epitaxial layer; fabricating P / N electrodes for electrical connection to the P-type and N-type semiconductor layers of the gallium nitride epitaxial layer, respectively; and fabricating a protective layer, exposing a portion of the electrodes for bonding wire encapsulation, while covering the remaining portion. Specifically, combining the photolithography of the MESA and TCL processes into one step allows for better control of the distance between them, significantly increasing the light-emitting area, effectively improving chip luminous efficiency, reducing fabrication steps, and increasing production capacity. Attached Figure Description

[0025] Figure 1 This is a flowchart illustrating the implementation of an LED chip fabrication method according to an embodiment of the present invention. Detailed Implementation

[0026] To facilitate understanding of the present invention, a more complete description will be given below with reference to the accompanying drawings. Several embodiments of the invention are illustrated in the drawings. However, the invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete.

[0027] It should be noted that when a component is said to be "fixed to" another component, it can be directly on the other component or there may be an intervening component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there may be an intervening component. The terms "vertical," "horizontal," "left," "right," and similar expressions used in this document are for illustrative purposes only.

[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0029] refer to Figure 1 The above is a flowchart illustrating an LED chip fabrication method according to an embodiment of the present invention. The method specifically includes the following steps:

[0030] S1: Provide a wafer substrate and perform PSS fabrication to obtain a PSS substrate;

[0031] S2: A gallium nitride epitaxial stack is fabricated on a PSS substrate, wherein the gallium nitride epitaxial stack includes a buffer layer, an N-type semiconductor layer, a light-emitting layer, and a P-type semiconductor layer sequentially deposited on the PSS substrate;

[0032] S3: An isolation trench region pattern is formed on the gallium nitride epitaxial stack using photolithography, and the gallium nitride epitaxial stack is etched until part of the PSS substrate is exposed.

[0033] Specifically, ISO (isolation zone) lithography can be a single photolithography process or a double photolithography process. A single photolithography process can be used for mid-to-low-end products that prioritize cost-effectiveness, saving costs. This involves one coating, exposure, and development cycle, resulting in the same ramp angle for all independent units of the high-voltage chip. A double photolithography process can be used for high-end products that prioritize high performance, achieving the ultimate light-emitting effect. This involves two coating, exposure, and development cycles, with an intermediate baking cycle. The angle at the electrode bridging points of the independent units of the high-voltage chip is gentler, which helps improve reliability, while the angles at other locations are more vertical, which helps maximize the utilization of the light-emitting area.

[0034] S4: The current blocking layer is fabricated in the region of the P-type semiconductor layer to reduce the recombination of charge carriers directly under the metal electrode and to prevent the radiated photons from being absorbed and blocked by the metal.

[0035] Specifically, the material of the current blocking layer is SiO2, and the thickness of the current blocking layer is 150nm to 420nm. N2 is used as the carrier gas, and N2O and SiH4 are used as the reactant gases. The ratio of reactant gases is 5 to 20:1, and the power is 50W to 100W. The current blocking layer is deposited on the substrate using a PECVD machine to obtain a dense and insulating current blocking layer.

[0036] S5: Fabricate a TCL film layer on the gallium nitride epitaxial stack and the current blocking layer, and form a MESA / TCL photolithographic pattern by photolithography.

[0037] Specifically, the TCL film material is either indium tin oxide or indium zinc oxide, and the thickness of the TCL film ranges from 25nm to 150nm. The TCL film deposition process is divided into two parts: the first layer is the contact layer, which is sputtered with lower power and a slower deposition rate; the second layer is the bulk layer, which is sputtered with higher power and a faster deposition rate. For example, using a sputtering evaporation machine, the sputtering power for the contact layer is 100W–180W, and the sputtering power for the bulk layer is 500W–700W. This difference is to reduce damage to the epitaxial layer from high-power sputtering.

[0038] S6: TCL is selectively etched through a single etching process, and then a second etching process is performed to expose the N-type semiconductor layer of the gallium nitride epitaxial stack.

[0039] Specifically, the first etching step is wet etching, and the second etching step is dry etching. During wet selective etching of the TCL film, the etching time is controlled to ensure that the distance between the TCL and the design pattern is 0μm to 1μm. Different etching times correspond to different film thicknesses. After wet etching, the wafer with adhesive is baked at a temperature of 60℃ to 90℃ for 35min to 50min to remove moisture. Then, ICP dry etching is performed using Cl2 as the etching gas.

[0040] After dry etching to remove the resist, the MESA differed from the design value by 1μm to 3μm. Ultimately, the actual distance between the MESA and the TCL was 3μm to 5μm, ensuring a safe distance between the two without wasting the light-emitting area.

[0041] S7: Prepare P / N electrodes for electrical connection with the P-type and N-type semiconductor layers of the gallium nitride epitaxial stack, respectively;

[0042] The thickness of both P / N electrodes is 2μm to 3.5μm.

[0043] S8: Prepare a protective layer, exposing part of the electrode to encapsulate the bonding wire, and covering the rest completely;

[0044] The protective layer is made of SiO2 and has a thickness of 60nm to 300nm.

[0045] The present invention will be further described below with reference to specific embodiments:

[0046] Example 1

[0047] The LED chip fabrication method in this embodiment includes the following steps:

[0048] (1) Provide a wafer substrate and perform PSS fabrication to obtain a PSS substrate;

[0049] (2) A gallium nitride epitaxial stack is prepared on a PSS substrate, wherein the gallium nitride epitaxial stack comprises a buffer layer, an N-type semiconductor layer, a light-emitting layer, and a P-type semiconductor layer sequentially deposited on the PSS substrate.

[0050] (3) An isolation trench region pattern is formed on the gallium nitride epitaxial stack by photolithography, and the gallium nitride epitaxial stack is etched until part of the PSS substrate is exposed.

[0051] Specifically, the ISO (isolation zone) lithography process uses two photolithography steps.

[0052] (4) The current blocking layer is fabricated in the region of the P-type semiconductor layer to reduce the recombination of charge carriers directly under the metal electrode and to prevent the radiated photons from being absorbed and blocked by the metal.

[0053] Specifically, the material of the current blocking layer is SiO2, and the thickness of the current blocking layer is 300nm. N2 is used as the carrier gas, and N2O and SiH4 are used as the reactant gases. The ratio of reactant gases is 10:1, and the power is 75W. The current blocking layer is deposited on the substrate using a PECVD machine to obtain a dense and insulating current blocking layer.

[0054] (5) A TCL film layer is fabricated on the gallium nitride epitaxial stack and the current blocking layer, and a MESA / TCL photolithographic pattern is formed by photolithography.

[0055] Specifically, the TCL film material is either indium tin oxide or indium zinc oxide, and the thickness of the TCL film is 100nm. The TCL film deposition is divided into two parts: the first layer is the contact layer, with lower sputtering power and slower deposition rate; the second layer is the bulk layer, with higher sputtering power and faster deposition rate. Taking a sputtering evaporation machine as an example, the sputtering power of the contact layer is 150W, and the sputtering power of the bulk layer is 600W. The difference between the two is to reduce damage to the epitaxial layer caused by high-power sputtering.

[0056] (6) TCL is selectively etched by wet etching and then dry etching is performed to expose the N-type semiconductor layer of the gallium nitride epitaxial stack.

[0057] Specifically, during wet selective etching of the TCL film, the etching time is controlled to ensure that the distance between the TCL and the design pattern is 0μm to 1μm. Different etching times correspond to different film thicknesses. After wet etching, the wafer with adhesive is baked at 80℃ for 40 minutes to remove moisture. Then, ICP dry etching is performed with Cl2 as the etching gas.

[0058] After dry etching to remove the resist, MESA differed from the design value by 1μm to 3μm. Ultimately, the actual distance between MESA and TCL was 3.1μm, ensuring a safe distance between the two without wasting the light-emitting area.

[0059] (7) Prepare P / N electrodes for electrical connection with the P-type semiconductor layer and N-type semiconductor layer of gallium nitride epitaxial stack, respectively;

[0060] The thickness of both the P and N electrodes is 2 μm.

[0061] (8) Prepare a protective layer, with the exposed part of the electrode used to encapsulate the bonding wire, and the rest completely covered;

[0062] The protective layer is made of SiO2 and has a thickness of 200 nm.

[0063] The final product was a 6-cell high-voltage chip with a size of approximately 17mil × 26mil.

[0064] Example 2

[0065] This second embodiment also provides an LED chip fabrication method. The difference from the first embodiment is that the final actual distance between MESA and TCL is 3.2μm.

[0066] Example 3

[0067] This third embodiment also provides an LED chip fabrication method. The difference from the first embodiment is that the final actual distance between MESA and TCL is 3.6μm.

[0068] Example 4

[0069] This fourth embodiment also provides an LED chip fabrication method. The difference from the first embodiment is that the final actual distance between MESA and TCL is 3.4μm.

[0070] Example 5

[0071] This fifth embodiment also provides an LED chip fabrication method. The difference from the first embodiment is that the final actual distance between MESA and TCL is 3.5μm.

[0072] Example 6

[0073] This sixth embodiment also provides an LED chip fabrication method. The difference from the first embodiment is that a three-string high-voltage chip with a size of approximately 12mil×20mil is finally fabricated, and the actual distance between MESA and TCL is 3.1μm.

[0074] Example 7

[0075] This seventh embodiment also provides an LED chip fabrication method. The difference from the sixth embodiment is that the final actual distance between MESA and TCL is 3.4μm.

[0076] Example 8

[0077] This embodiment eight also provides an LED chip fabrication method. The difference from embodiment six is ​​that the final actual distance between MESA and TCL is 3.5μm.

[0078] Example 9

[0079] This embodiment nine also provides an LED chip fabrication method. The difference from embodiment six is ​​that the final actual distance between MESA and TCL is 3.3 μm.

[0080] Example 10

[0081] This tenth embodiment also provides an LED chip fabrication method. The difference from the sixth embodiment is that the final actual distance between MESA and TCL is 3.3μm.

[0082] The LED chips prepared in Examples 1 to 10 were tested under the same conditions, and the specific results are as follows:

[0083]

[0084]

[0085] As can be seen from the table, the LED chips obtained by the method in the embodiments of the present invention have improved luminous brightness to varying degrees compared with LED chips prepared by conventional processes, under the same test conditions.

[0086] This invention also provides an LED chip, which is prepared by the above-described LED chip preparation method. Specifically, the actual distance between MESA and TCL is 3μm to 5μm.

[0087] In summary, the LED chip and its fabrication method in this embodiment of the invention include providing a semi-finished LED chip, which comprises a PSS substrate and a gallium nitride epitaxial layer and a current blocking layer sequentially deposited on the PSS substrate; fabricating a TCL film layer on the gallium nitride epitaxial layer and the current blocking layer, and forming a MESA / TCL photolithographic pattern using photolithography; selectively etching the TCL layer through a first etching step, followed by a second etching step to expose the N-type semiconductor layer of the gallium nitride epitaxial layer; fabricating P / N electrodes for electrical connection to the P-type and N-type semiconductor layers of the gallium nitride epitaxial layer, respectively; and fabricating a protective layer, exposing a portion of the electrodes for bonding wire encapsulation, while covering the remaining portion. Specifically, combining the photolithography of the MESA and TCL processes into one step allows for better control of the distance between them, significantly increases the light-emitting area, effectively improves the chip's luminous efficiency, reduces fabrication steps, and increases production capacity.

[0088] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these modifications and improvements all fall within the scope of protection of the present invention. Therefore, the scope of protection of this patent should be determined by the appended claims.

Claims

1. A method for fabricating an LED chip, characterized in that, The method includes: A semi-finished LED chip is provided, the semi-finished LED chip comprising a PSS substrate, and a gallium nitride epitaxial stack and a current blocking layer sequentially deposited on the PSS substrate; A TCL film layer was fabricated on the gallium nitride epitaxial stack and the current blocking layer, and a MESA / TCL photolithographic pattern was formed by photolithography. TCL is selectively etched in one etching process, and then a second etching process is used to expose the N-type semiconductor layer of the gallium nitride epitaxial stack. P / N electrodes are fabricated for electrical connection to the P-type and N-type semiconductor layers of a gallium nitride epitaxial stack, respectively. Prepare a protective layer, exposing part of the electrode to encapsulate the bonding wire, and covering the rest completely; The step of providing a semi-finished LED chip, the semi-finished LED chip comprising a PSS substrate, and a gallium nitride epitaxial layer and a current blocking layer sequentially deposited on the PSS substrate, includes: A wafer substrate is provided, and PSS fabrication is performed to obtain a PSS substrate; Gallium nitride epitaxial stacks are fabricated on PSS substrates, wherein the gallium nitride epitaxial stacks include a buffer layer, an N-type semiconductor layer, a light-emitting layer, and a P-type semiconductor layer sequentially deposited on the PSS substrates. The isolation trench region pattern is formed on the gallium nitride epitaxial stack using photolithography, and the gallium nitride epitaxial stack is etched until part of the PSS substrate is exposed. The current blocking layer is fabricated in the region of the P-type semiconductor layer to reduce the recombination of charge carriers directly below the metal electrode and to prevent the radiated photons from being absorbed and blocked by the metal.

2. The LED chip fabrication method according to claim 1, characterized in that, In the step of selectively etching TCL through a first etching and then exposing the N-type semiconductor layer of the gallium nitride epitaxial stack through a second etching, the actual distance between MESA and TCL is 3μm~5μm.

3. The LED chip fabrication method according to claim 2, characterized in that, In the step of selectively etching the TCL through a first etching and then exposing the N-type semiconductor layer of the gallium nitride epitaxial stack through a second etching, the actual etched TCL has a spacing of 0μm~1μm compared with the TCL design pattern.

4. The LED chip fabrication method according to claim 3, characterized in that, In the step of selectively etching the TCL through a first etching and then exposing the N-type semiconductor layer of the gallium nitride epitaxial stack through a second etching, the actual etched MESA has a spacing of 1μm to 3μm compared with the MESA design pattern.

5. The LED chip fabrication method according to claim 4, characterized in that, The material of the current blocking layer is SiO2, and the thickness of the current blocking layer is 150nm~420nm.

6. The LED chip fabrication method according to claim 5, characterized in that, The material of the TCL film is either indium tin oxide or indium zinc oxide, and the thickness of the TCL film is 25nm~150nm.

7. The LED chip fabrication method according to claim 1, characterized in that, The first etching is wet etching, and the second etching is dry etching.

8. An LED chip, characterized in that, The LED chip is prepared according to any one of claims 1 to 7.

9. The LED chip according to claim 8, characterized in that, The actual distance between MESA and TCL is 3μm~5μm.

Citation Information

Patent Citations

  • LED (Light Emitting Diode) surface patch type encapsulating structure based on silicon base plate and encapsulating method thereof

    CN101997074A

  • Method of manufacturing semiconductor light emitting element

    JP2011199122A