Preparation method of a double transition metal electrocatalyst, lithium-sulfur battery and application thereof
By preparing a sheet-like graphene-like dual transition metal electrocatalyst, the kinetics and stability issues of lithium-sulfur batteries were solved, the charge-discharge performance and cycle life of the batteries were improved, and the application of efficient lithium-sulfur battery cathode materials was realized.
Patent Information
- Application Number
- CN202410096984.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-23
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-01-23
AI Technical Summary
Lithium-sulfur batteries suffer from problems such as volume expansion, slow reaction kinetics, short cycle life, poor conductivity, and the 'shuttle effect' caused by the dissolution of polysulfides, which limit their commercial application.
A dual-transition metal electrocatalyst preparation method was adopted, which combined chemical solution method with high-temperature calcination method to prepare a catalyst with a sheet-like graphene-like structure. The catalyst was mixed with sulfur and used as a positive electrode material for lithium-sulfur batteries. Nitrogen-doped carbon materials were used to improve catalytic activity and conductivity, and metal elements were introduced to regulate electronic structure and active sites.
It significantly improves the reaction kinetics and cycle stability of lithium-sulfur batteries, enhances battery charge-discharge efficiency and lifespan, reduces production costs, and has industrialization potential.
Smart Images

Figure CN117936785B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of battery catalyst materials, specifically relating to a dual transition metal electrocatalyst for lithium-sulfur batteries and its preparation method. Background Technology
[0002] Developing lithium-ion battery cathode materials with high redox potential, high material packing density, good stability, high conductivity, low production cost, and simple manufacturing process is of epoch-making significance for solving increasingly serious energy and environmental problems. Currently, lithium-sulfur batteries, due to their high theoretical capacity (1675 mAh / g) as conversion-type cathode materials, have significant advantages as next-generation lithium battery cathode materials, mainly reflected in their high theoretical energy density, relatively low cost, and relatively environmentally friendly characteristics.
[0003] However, lithium-sulfur batteries still suffer from problems such as volume expansion, slow reaction kinetics, short cycle life, poor conductivity, and the "shuttle effect" caused by polysulfide dissolution. These issues limit the commercial application of lithium-sulfur batteries. Electrocatalysts can accelerate the redox process of lithium-sulfur batteries, solve the polysulfide "shuttle effect" problem, and significantly improve the electrochemical performance of lithium-sulfur batteries.
[0004] CN115986125B discloses a two-dimensional transition metal sulfide catalyst and a lithium-sulfur battery based thereon. The catalyst is prepared by dispersing MnS2 powder in N,N-dimethylformamide solvent and subjecting it to ultrasonic cavitation to obtain a dispersion containing ultrathin MnS2 nanosheets. The dispersion solution is centrifuged to obtain a supernatant, which is then vacuum filtered to obtain ultrathin MnS2 nanosheets. The ultrathin MnS2 nanosheets obtained in step S2 are characterized by X-ray diffraction. Based on the characteristics of the XRD pattern, ultrathin MnS2 nanosheets with quasi-crystalline orientation are selected, which constitute the two-dimensional transition metal sulfide catalyst. This catalyst material has dual adsorption-catalysis functions, exhibiting strong adsorption of soluble lithium polysulfides and excellent catalytic activity in the charge-discharge reaction process of lithium-sulfur batteries. It effectively alleviates the shuttle effect of lithium polysulfides in lithium-sulfur batteries, thereby enabling the lithium-sulfur battery to exhibit excellent electrochemical performance during cycling.
[0005] This patent explains the catalytic effect by describing the characteristics of the material itself, combined with active sites and reaction kinetics, but does not address its application in lithium-sulfur batteries. This patent, however, explains the catalytic effect based on the electrochemical performance of lithium-sulfur batteries; the two are fundamentally different. Secondly, the manganese sulfide invented in this patent belongs to the metal sulfide catalyst class. The working principle of metal sulfide lithium-sulfur battery cathode materials involves the insertion and extraction of lithium ions, as well as the electrochemical reaction with the intercalation compounds formed with sulfides. This patent's cathode is sulfur, but it is doped with a catalyst to promote the reaction between sulfur and lithium ions. There are also significant differences in electrochemical performance, such as charge / discharge voltage range and capacity. Summary of the Invention
[0006] This invention aims to solve the problems of the prior art mentioned above. It proposes a method for preparing a dual-transition metal electrocatalyst, a lithium-sulfur battery, and its applications. The technical solution of this invention is as follows:
[0007] A method for preparing a dual transition metal electrocatalyst, comprising the following steps:
[0008] Dicyandiamide and glucose were dissolved in deionized water at a mass ratio of 20:1.
[0009] Ammonium molybdate and ammonium chromate in a molar ratio of 1:1 were dissolved in deionized water and added dropwise to a deionized aqueous solution of dicyandiamide and glucose. The solution was heated in an oil bath at 80°C for 2 hours under an argon atmosphere to obtain a light green clear solution.
[0010] The solution was freeze-dried to obtain a light green flocculent, which was then calcined at 600°C for 2 hours and 900°C for 2 hours under an argon atmosphere to obtain a dual transition metal electrocatalyst.
[0011] Furthermore, the step of dissolving dicyandiamide and glucose in deionized water at a mass ratio of 20:1 specifically includes:
[0012] Dissolve 5g of dicyandiamide and 0.25g of glucose in 290ml of deionized water.
[0013] Furthermore, the process of dissolving ammonium molybdate and ammonium chromate in deionized water at a molar ratio of 1:1 specifically includes:
[0014] Dissolve 0.0076 mg ammonium chromate and 0.0088 mg ammonium molybdate in 10 ml of deionized water in a beaker.
[0015] Furthermore, the heating rate for calcining at 600°C for 2 hours and at 900°C for 2 hours under an argon atmosphere is 3°C / min.
[0016] A lithium-sulfur battery, wherein the positive electrode material of the lithium-sulfur battery is a mixture of any one of the dual transition metal electrocatalysts and sulfur, heated in an argon atmosphere at 155°C.
[0017] The application of a dual transition metal electrocatalyst in lithium-sulfur batteries includes the following steps:
[0018] (1) The obtained dual transition metal electrocatalyst was mixed with sulfur in a mortar at a ratio of 2:8, transferred to a reaction vessel, and heated in an argon atmosphere at 155°C for 12 hours to obtain sulfur cathode material.
[0019] (2) Mix sulfur cathode material: conductive carbon black: binder in a ratio of 8:1:1. Add a certain amount of NMP (N-methylpyrrolidone) to the mixture and stir for 12 hours before coating it onto the surface of aluminum foil.
[0020] (3) Place the coated electrode in a vacuum drying oven at 60°C for 12 hours to allow the electrode to dry completely;
[0021] (4) Use a cutting machine to cut the electrode into round pieces with a diameter of 12mm, and weigh the electrode;
[0022] (5) Assemble the positive electrode shell, the positive electrode sheet obtained in step (4), 50 μL of lithium-sulfur electrolyte, polypropylene separator, gasket, and negative electrode shell into a battery in sequence. The sulfur loading of the positive electrode sheet is 1.2 mg / cm³. 2 .
[0023] The advantages and beneficial effects of this invention are as follows:
[0024] According to the present invention, a dual transition metal electrocatalyst for lithium-sulfur batteries and its preparation method are disclosed. The dual transition metal electrocatalyst is prepared by a combination of a chemical solution method and a high-temperature calcination method. When applied to the cathode material of lithium-sulfur batteries, the catalyst exhibits high rate performance and long cycle life, significantly improving the reaction kinetics during the charge-discharge process of lithium-sulfur batteries. Furthermore, the lithium-sulfur battery catalyst of the present invention is low in production cost, has a simple manufacturing process, and is environmentally friendly and pollution-free, making it of significant practical importance and possessing great potential for further industrialization.
[0025] In lithium-sulfur batteries, the heterogeneous reactions of sulfur and intermediate products in the electrochemical process can lead to a decline in battery performance. Therefore, introducing catalysts to promote sulfur reactions is a common strategy. This invention introduces nitrogen atoms into carbon materials through nitrogen doping, altering the electronic structure of carbon and thereby enhancing its catalytic activity, which helps improve the performance of lithium-sulfur batteries. The introduction of metal elements can further modulate the electronic structure and chemical properties of carbon materials, improve conductivity, and thus facilitate more efficient electron conduction. Furthermore, metal elements can introduce new active sites, which help catalyze sulfur reactions, further improving the cycle stability and electrochemical performance of the battery. Attached Figure Description
[0026] Figure 1 These are TEM images of the lithium-sulfur battery catalyst material provided by a preferred embodiment of the present invention. 1a shows the microstructure of the dual transition metal electrocatalyst material, which is a sheet-like graphene-like structure. 1b shows the corresponding element mapping.
[0027] Figure 2 a is the cycling curve of a lithium-sulfur battery using the catalyst material in an embodiment of the present invention at a rate of 0.2C, and 2b is the cycling curve at a rate of 1C.
[0028] Figure 3 a is the cycling curve of a lithium-sulfur battery using the catalyst material in an embodiment of the present invention under different rate conditions, and 3b is the cyclic voltammetry curve at different scan rates.
[0029] Figure 4 This is a flowchart illustrating the preparation process of the dual transition metal electrocatalyst of the present invention. Detailed Implementation
[0030] The technical solutions of the present invention will be clearly and thoroughly described below with reference to the accompanying drawings. The described embodiments are merely some embodiments of the present invention.
[0031] The technical solution of the present invention to solve the above-mentioned technical problems is:
[0032] A method for preparing a dual transition metal electrocatalyst, comprising the following steps:
[0033] Dicyandiamide and glucose were dissolved in deionized water at a mass ratio of 20:1.
[0034] Ammonium molybdate and ammonium chromate in a molar ratio of 1:1 were dissolved in deionized water and slowly added dropwise to the solution in step (1). The solution was heated in an oil bath at 80°C for 2 hours under an argon atmosphere to obtain a light green clear solution. The solution was freeze-dried to obtain a light green flocculent, which was then calcined at 600°C for 2 hours and 900°C for 2 hours under an argon atmosphere to obtain a dual transition metal electrocatalyst.
[0035] This invention provides a method for preparing a dual transition metal electrocatalyst, which can be used in the field of lithium-sulfur batteries, particularly addressing the problems of slow reaction kinetics and poor cycle stability at the sulfur electrode in lithium-sulfur batteries. The synthesis process of the lithium-sulfur battery catalyst material in the embodiments of the invention includes the following steps: 5g of dicyandiamide and 0.25g of glucose are dissolved in 290ml of deionized water in a three-necked flask; then 0.0076mg of ammonium chromate and 0.0088mg of ammonium molybdate are dissolved in 10ml of deionized water in a beaker, and then slowly added dropwise to the three-necked flask. Under argon protection, the temperature is raised to 80℃, and the reaction is carried out for 2 hours. After cooling, the solution is freeze-dried to obtain a light green flocculent, which is then calcined at 600℃ for 2 hours and 900℃ for 2 hours under an argon atmosphere, with a heating rate of 3℃ / min. This yields the dual transition metal electrocatalyst. The positive electrode, negative electrode, electrolyte, and separator of this invention are prepared according to methods commonly used by those skilled in the art (therefore, they are not described in detail here).
[0036] The application of the dual transition metal electrocatalyst material in the above embodiment on lithium-sulfur batteries is as follows: (1) The catalyst obtained above is mixed with sulfur in a mortar at a ratio of 2:8, transferred to a reaction vessel, and heated in an argon atmosphere at 155°C for 12 hours to obtain sulfur cathode material; (2) Sulfur cathode material: conductive carbon black: binder are mixed evenly at a ratio of 8:1:1, a certain amount of NMP (N-methylpyrrolidone) is added to the mixture, and after stirring for 12 hours, it is coated onto the surface of aluminum foil; (3) The coated electrode is placed in a vacuum drying oven at 60°C and kept warm for 12 hours to allow the electrode to dry fully; (4) The electrode is cut into round pieces with a diameter of 12 mm using a cutting machine, and the mass of the electrode is weighed. (5) The positive electrode shell, the positive electrode sheet obtained in step (4), 50 μL of lithium-sulfur electrolyte, polypropylene separator, gasket and negative electrode shell are assembled into a battery in sequence, and the sulfur loading of the positive electrode sheet is 1.2 mg / cm³. 2 .
[0037] Depend on Figure 1 It is evident that the microstructure of the dual transition metal electrocatalytic material is a sheet-like graphene-like structure. The images show that individual Cr / Mo alloy nanoparticles are uniformly distributed on the nitrogen-doped graphene nanosheets without obvious aggregation, exhibiting clear lattice fringes. Nitrogen-doped graphene, as a substrate, provides excellent conductivity and specific surface area. The introduction of the Cr / Mo alloy dual transition metals provides a large number of active sites, effectively accelerating the conversion of polysulfides and effectively suppressing the "shuttle effect" in lithium-sulfur batteries.
[0038] After electrochemical performance testing Figure 2a shows the long-cycle charge-discharge curve under 0.2C rate conditions. The discharge capacity in the first cycle is close to 1400mAh / g, and after 100 cycles, the capacity is still maintained at 1200mAh / g, with a capacity decay rate of only 0.154%.
[0039] Figure 2 b shows the long-cycle charge-discharge curve under 1C rate conditions. The initial discharge capacity is 820mAh / g, and after 500 cycles, the capacity remains at 580mAh / g, with a capacity decay rate of only 0.345%.
[0040] Figure 3 a shows the charge-discharge curves under 0.2C, 0.5C, 1C, 2C, 5C, and 10C conditions. It can be seen that under the high rate of 5C, the battery discharge capacity is 700mAh / g, and even under the high rate of 10C, the battery discharge capacity is still 440mAh / g. After returning to the low rate conditions, the battery capacity can still maintain a similar level as before.
[0041] Figure 3 b shows the cyclic voltammetry curves at different scan rates, all of which exhibit strong redox peaks.
[0042] Electrochemical performance tests showed that the lithium-sulfur battery loaded with dual transition metal electrocatalysts significantly improved the conductivity of the sulfur electrode, effectively suppressed the "shuttle effect" of the lithium-sulfur battery, exhibited good cycle stability, and demonstrated excellent rate performance.
[0043] It should also be noted that the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitation, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.
[0044] The above embodiments should be understood as illustrative only and not as limiting the scope of protection of the present invention. After reading the description of the present invention, those skilled in the art can make various alterations or modifications to the present invention, and these equivalent changes and modifications also fall within the scope defined by the claims of the present invention.
Claims
1. A method for preparing a dual transition metal electrocatalyst for lithium-sulfur batteries, characterized in that, Includes the following steps: Place 5 g of dicyandiamide and 0.25 g of glucose in a three-necked flask and add 290 ml of deionized water to dissolve them; Dissolve 0.0076 mg of ammonium chromate and 0.0088 mg of ammonium molybdate in 10 ml of deionized water in a beaker. It was then added dropwise to the aforementioned deionized aqueous solution of dicyandiamide and glucose, and heated in an oil bath at 80°C for 2 hours under an argon atmosphere to obtain a light green clear solution. The solution was freeze-dried to obtain a light green flocculent, which was then calcined at 600°C for 2 hours and 900°C for 2 hours under an argon atmosphere to obtain a dual transition metal electrocatalyst.
2. The method for preparing the dual transition metal electrocatalyst for lithium-sulfur batteries according to claim 1, characterized in that, The heating rate for calcining at 600℃ for 2 hours and at 900℃ for 2 hours under an argon atmosphere is 3℃ / min.
3. A lithium-sulfur battery, characterized in that, The positive electrode material of the lithium-sulfur battery is prepared by mixing a dual transition metal electrocatalyst prepared by any one of claims 1 to 2 with sulfur and heating it in an argon atmosphere at 155°C.
4. The application of a dual transition metal electrocatalyst prepared by the method of claim 1 in a lithium-sulfur battery, characterized in that, Includes the following steps: (1) The obtained dual transition metal electrocatalyst and sulfur were mixed evenly in a mortar at a ratio of 2:8, transferred to a reaction vessel, and heated in an argon atmosphere at 155°C for 12 h to obtain sulfur cathode material; (2) Mix sulfur cathode material: conductive carbon black: binder in a ratio of 8:1:
1. Add a certain amount of N-methylpyrrolidone to the mixture, stir for 12 hours and then apply it to the surface of aluminum foil. (3) Place the coated electrode in a vacuum drying oven at 60°C for 12 hours to allow the electrode to dry completely; (4) Use a cutting machine to cut the electrode into round pieces with a diameter of 12 mm, and weigh the electrode; (5) Assemble the positive electrode shell, the positive electrode sheet obtained in step (4), 50 μL of lithium-sulfur electrolyte, polypropylene separator, gasket, and negative electrode shell into a battery in sequence. The sulfur loading of the positive electrode sheet is 1.2 mg / cm³. 2 .
Citation Information
Patent Citations
Cathode material used for lithium sulfur battery, preparation and application thereof
CN105322189A
Preparation method of high-entropy alloy used as lithium-sulfur battery catalytic material
CN115084527A
Preparation method and application of supported copper-chromium catalyst
CN117085722A