Process for the preparation of an electrolyte additive composition and electrolyte composed thereof
By generating a composition of lithium tri(boron trifluoride)phosphate and lithium (difluorophosphoryloxy)trifluoroborate, the problem of boron trifluoride residue was solved, and the stability of the electrolyte and the performance of the battery were improved.
Patent Information
- Application Number
- CN202211253325.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-13
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-10-13
AI Technical Summary
In the prior art, it is difficult to completely remove boron trifluoride residue during the preparation of lithium tri(boron trifluoride) phosphate, which leads to increased discoloration of the electrolyte and damage to the stability of the interfacial film, thus deteriorating the battery's cycle and storage performance.
A composition of lithium tri(boron trifluoride) phosphate and lithium (difluorophosphoryloxy)trifluoroborate was generated by reacting boron trifluoride and lithium phosphate. The residual boron trifluoride was completely removed by adding lithium difluorophosphate, and the molar ratio was adjusted to obtain the optimal composition.
Completely removes boron trifluoride residue, improves electrolyte storage stability, and enhances battery high and low temperature performance and cycle performance.
Smart Images

Figure QLYQS_1 
Figure BDA0003888657870000021 
Figure BDA0003888657870000022
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion battery electrolytes, and particularly to a method for preparing an electrolyte additive composition of lithium tri(boron trifluoride)phosphate and lithium (difluorophosphoryloxy)trifluoroborate, and an electrolyte comprising the prepared additive composition. Background Technology
[0002] Electrolyte additives are an indispensable component of lithium-ion batteries. They are mainly responsible for building a stable electrode / electrolyte interface film to achieve electronic insulation and facilitate lithium-ion transport. Under the influence of different functional groups in the additives, the composition and structure of the battery interface film are changed, which ultimately affects battery performance such as battery cycle life, high-temperature storage, and low-temperature discharge.
[0003] Boron-containing additives, due to the electron-deficient effect of boron atoms, can dissolve inorganic lithium salts such as LiF on the surface of the interfacial film. Therefore, adding an appropriate amount of boron-containing additives can reduce the internal resistance of the battery and improve its low-temperature performance. Phosphorus-containing additives, such as phosphate esters and phosphates, have strong interactions between the "P=O" in their components and the transition metal elements on the positive electrode surface, thereby forming a stable positive electrode interfacial film on the surface, improving the battery's storage and cycle performance. In addition, phosphorus-containing additives have a certain flame-retardant effect in the electrolyte. When phosphorus and boron are both present in an additive, they can simultaneously possess the above-mentioned advantageous properties.
[0004] Patent CN105103361A discloses a compound containing both phosphorus and boron, including lithium tri(boron trifluoride)phosphate. Using this compound as an electrolyte additive can reduce the initial impedance of the battery and improve the initial coulombic efficiency and initial discharge capacity. Lithium tri(boron trifluoride)phosphate is prepared by reacting lithium phosphate with a diethyl carbonate solution of boron trifluoride. During the reaction, excess boron trifluoride is added to ensure complete reaction, and then the excess boron trifluoride is removed by vacuum distillation. However, vacuum distillation cannot completely remove boron trifluoride from the system; the residual amount is generally around 10 wt%. This residual boron trifluoride not only causes a red shift in the spectrum due to its strong Lewis acidity catalyzing the polymerization of unsaturated carbonates in the electrolyte, leading to increased electrolyte discoloration, but also excessively dissolves inorganic salt components in the interfacial film, damaging the interfacial film stability and thus deteriorating the battery's cycle performance and storage performance.
[0005] Therefore, in order to better utilize lithium tri(boron trifluoride) phosphate in the electrolyte, it is necessary to reduce the residual amount of boron trifluoride in lithium tri(boron trifluoride) phosphate. Summary of the Invention
[0006] To address the aforementioned technical problems, this invention proposes a method for preparing an electrolyte additive composition comprising lithium tri(boron trifluoride)phosphate and lithium (difluorophosphoryloxy)trifluoroborate, wherein no boron trifluoride residue is found in the composition.
[0007] The objective of this invention is achieved through the following technical solution:
[0008] A method for preparing an electrolyte additive composition comprising lithium tri(boron trifluoride)phosphate and lithium (difluorophosphoryloxy)trifluoroborate, the method comprising:
[0009] (1) An intermediate solution is obtained by reacting lithium phosphate and boron trifluoride, wherein the molar ratio of boron trifluoride to lithium phosphate is (3.5-6.0):1;
[0010] (2) Lithium difluorophosphate is added to the intermediate solution, and the mixture is reacted at 5–90°C for 0.2–24 h to obtain a composition of lithium tri(boron trifluoride) phosphate as shown in formula (A) and lithium (difluorophosphoryloxy)trifluoroborate as shown in formula (B):
[0011]
[0012] The molar ratio of lithium difluorophosphate to lithium phosphate is (0.5-3):1.
[0013] In step (1), lithium phosphate and boron trifluoride react to obtain lithium tri(boron trifluoride)phosphate as shown in formula (A) above, and the reaction formula is as follows:
[0014]
[0015] Since lithium phosphate has extremely low solubility in organic solvents, maintaining a boron trifluoride / lithium phosphate molar ratio greater than 3 / 1 in actual operation yields the best reaction results, such as (3.5-6.0):1, and more preferably (3.5-4.5):1.
[0016] In step (2), excess boron trifluoride from step (1) is removed by adding lithium difluorophosphate, and lithium (difluorophosphoryloxy)trifluoroborate as shown in formula (B) above is also obtained, with the following reaction formula:
[0017]
[0018] Specifically, in step (1), lithium phosphate and boron trifluoride gas or boron trifluoride complex react in the presence of a reaction solvent to obtain an intermediate solution, or lithium phosphate and boron trifluoride complex react to obtain an intermediate solution; the reaction temperature is 5-90°C, and the reaction time is 0.2-24h; preferably the reaction temperature is 25-60°C, and preferably the reaction time is 0.5-6h.
[0019] Furthermore, the boron trifluoride complex is selected from at least one of the following: boron trifluoride dimethyl carbonate complex, boron trifluoride diethyl ether complex, boron trifluoride dimethyl ether complex, boron trifluoride butyl ether complex, boron trifluoride ethyl acetate complex, boron trifluoride sulfolane complex, and boron trifluoride tetrahydrofuran complex.
[0020] The reaction solvent is selected from at least one of dimethyl carbonate, methyl ethyl carbonate, diethyl carbonate, acetonitrile, or diethyl ether. Preferably, the reaction solvent is selected from commonly used non-aqueous solvents in electrolytes, such as dimethyl carbonate, methyl ethyl carbonate, and diethyl carbonate, so that the electrolyte additive composition obtained in this way can be used for electrolyte preparation without further treatment. Of course, the obtained additive composition can also be concentrated by methods such as vacuum distillation without affecting its use.
[0021] In step (2), excess boron trifluoride is removed by adding lithium difluorophosphate. The preferred reaction temperature is 25–60°C, and the preferred reaction time is 0.5–6 h.
[0022] The above method can completely remove residual boron trifluoride from lithium tri(boron trifluoride)phosphate. The residual amount of boron trifluoride can be determined using nuclear magnetic resonance spectroscopy.
[0023] In the additive composition obtained by this invention, the ratio of lithium tri(boron trifluoride)phosphate to lithium (difluorophosphoryloxy)trifluoroborate is related to the amount of lithium phosphate and boron trifluoride used. Different ratios of lithium tri(boron trifluoride)phosphate and lithium (difluorophosphoryloxy)trifluoroborate can be obtained by adjusting the amounts of lithium phosphate and boron trifluoride. Specifically, the molar ratio of boron trifluoride to lithium phosphate is between 3.5 / 1 and 6 / 1. The optimal amount of lithium (difluorophosphate) added is: (molar amount of boron trifluoride added - molar amount of lithium phosphate added) × 3. The final composition of lithium tri(boron trifluoride)phosphate and lithium (difluorophosphoryloxy)trifluoroborate has a molar ratio between 2 / 1 and 1 / 3.
[0024] Of course, the amount of lithium difluorophosphate added can also be greater than the above-mentioned optimal amount, but the composition obtained in this case will contain lithium difluorophosphate in addition to lithium tri(boron trifluoride)phosphate and lithium (difluorophosphoryloxy)trifluoroborate.
[0025] The present invention also provides a lithium-ion battery electrolyte comprising a main lithium salt and a non-aqueous solvent, wherein the electrolyte further comprises an additive composition containing lithium tri(boron trifluoride)phosphate and lithium (difluorophosphoryloxy)trifluoroborate obtained by any of the above preparation methods.
[0026] Specifically, in the electrolyte, lithium tri(boron trifluoride) phosphate accounts for 0.01% to 10% of the total mass of the electrolyte, lithium (difluorophosphoryloxy)trifluoroborate accounts for 0.01% to 10% of the total mass of the electrolyte, and the mass ratio of lithium tri(boron trifluoride) phosphate to lithium (difluorophosphoryloxy)trifluoroborate is (3.64 to 0.61):1.
[0027] Preferably, lithium tri(boron trifluoride) phosphate accounts for 0.2% to 5.0% of the total mass of the electrolyte, and lithium (difluorophosphoryloxy)trifluoroborate accounts for 0.2% to 5.0% of the total mass of the electrolyte.
[0028] In practice, the composition of the present invention can be directly used in the preparation of electrolytes. Therefore, from the perspective of the composition, the amount of the composition added (the total amount of lithium tri(boron trifluoride)phosphate and lithium (difluorophosphoryloxy)trifluoroborate) accounts for 0.4% to 10.0% of the total mass of the electrolyte, more preferably 1.0% to 7.0%, wherein the ratio of lithium tri(boron trifluoride)phosphate and lithium (difluorophosphoryloxy)trifluoroborate can be adjusted by adjusting the amount of raw materials added during the preparation process.
[0029] In the electrolyte of the present invention, the main lithium salt is selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethylsulfonyl)imide, and its molar concentration is 0.1 to 4.0 mol / L, more preferably 0.8 to 1.5 mol / L.
[0030] The organic solvent used in this invention can be any commonly used organic solvent in electrolytes. Preferably, the organic solvent is selected from at least one of C3-C6 carbonate compounds, C3-C8 carboxylic acid ester compounds, sulfone compounds, and ether compounds. Further, the C3-C6 carbonate compounds are selected from at least one of ethylene carbonate, propylene carbonate, butenyl carbonate, dimethyl carbonate, methyl ethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, and ethyl propyl carbonate; the C3-C8 carboxylic acid ester compounds are selected from at least one of γ-butyrolactone, methyl acetate, methyl propionate, methyl butyrate, ethyl acetate, ethyl propionate, ethyl butyrate, propyl acetate, and propyl propionate; the sulfone compounds are selected from at least one of sulfolane, dimethyl sulfoxide, dimethyl sulfone, and diethyl sulfone; and the ether compounds are selected from triethylene glycol dimethyl ether and / or tetraethylene glycol dimethyl ether.
[0031] Furthermore, to further improve the overall performance of the battery, the electrolyte also includes at least one of the following: vinylene carbonate, 1,3-propanesulfonate lactone, vinyl sulfate, 4-methyl vinyl sulfate, 4,4'-divinyl sulfate, ethyl fluorocarbonate, difluorovinyl carbonate, tris(trimethylsilane) phosphate, tris(trimethylsilane) borate, lithium difluorophosphate, lithium difluorosulfonylimide, lithium difluorobis(oxalate) phosphate, and lithium difluorooxalate borate, with any one of them added accounting for 0.1 wt% to 5.0 wt% of the total mass of the electrolyte.
[0032] In particular, the presence of vinylene carbonate and / or 1,3-propanesulfonate lactone in the electrolyte further enhances battery performance. For example, when vinylene carbonate is further added to the electrolyte, the content of inorganic salt components at the battery interface increases under the action of the composition, reducing the amount of vinylene carbonate required for film formation. Therefore, it does not significantly increase the initial impedance of the battery. On the other hand, the formation of an interfacial film rich in both inorganic salts and organic polymers simultaneously enhances the ionic conductivity and electronic insulation of the interfacial film, thus further improving cycle performance. Similarly, when 1,3-propanesulfonate lactone is further added to the electrolyte, it not only further suppresses battery gas production but also does not worsen the initial impedance or impedance growth during storage.
[0033] The present invention also provides a lithium-ion battery, comprising a positive electrode, a negative electrode, a separator, and an electrolyte as described above.
[0034] The active material of the positive electrode is selected from nickel-cobalt-manganese ternary materials, nickel-cobalt-aluminum ternary materials, lithium cobalt oxide materials, or lithium iron phosphate materials; wherein, the nickel-cobalt-manganese ternary material is Li(NixCoyMnz)O2, x≥0.5, y>0, z>0, x+y+z=1; the nickel-cobalt-aluminum ternary material is Li(NixCoyAlz)O2, x≥0.8, y>0, z>0, x+y+z=1.
[0035] The active material of the negative electrode is graphite, silicon suboxide, silicon, lithium metal, or a composite material thereof.
[0036] The separator is selected from commonly used separators in lithium-ion batteries.
[0037] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0038] 1. This invention removes boron trifluoride from lithium tri(boron trifluoride) phosphate by adding lithium difluorophosphate. This not only simplifies the operation but also completely removes residual boron trifluoride, preventing battery performance degradation and improving electrolyte storage stability.
[0039] 2. The present invention proposes an electrolyte additive composition of lithium tri(boron trifluoride) phosphate and lithium (difluorophosphoryloxy)trifluoroborate by adjusting the amount of lithium phosphate and boron trifluoride to remove boron trifluoride residue. When this composition is applied to the electrolyte, it can improve the high and low temperature performance of the battery at the same time compared with the use of lithium tri(boron trifluoride) phosphate or lithium (difluorophosphoryloxy)trifluoroborate alone. Detailed Implementation
[0040] The present invention will be further described below with reference to specific embodiments, but the invention is not limited to these specific embodiments. Those skilled in the art should recognize that the present invention covers all alternatives, improvements, and equivalents that may be included within the scope of the claims.
[0041] I. Implementation Examples
[0042] Example 1
[0043] This embodiment provides a method for preparing an electrolyte additive composition, specifically including the following steps:
[0044] S1. In a drying room with a dew point of -40℃, add 0.05 mol of lithium phosphate (99% purity) to the reaction flask, add dimethyl carbonate as a solvent, and start stirring to mix the system evenly; then introduce 0.18 mol of boron trifluoride gas into the reaction flask and react at 25℃ for 1 h to obtain an intermediate solution.
[0045] S2. Add 0.025 mol of lithium difluorophosphate to the intermediate solution and react at 25°C for 0.5 h to obtain an additive composition containing lithium tri(boron trifluoride) phosphate (referred to as compound A) and lithium (difluorophosphoryloxy)trifluoroborate (referred to as compound B), referred to as composition 1#.
[0046] NMR analysis showed that the nuclear magnetic resonance... 19 The F spectrum is shown below:
[0047] Compound A: δ = -159.06 ppm(s)
[0048] Compound B: δ = -87.44 ppm (d, J = 10¹² Hz)
[0049] Boron trifluoride: None
[0050] The results showed that no boron trifluoride residue was found in composition 1#. (NMR analysis was performed.) 19 Integrating the F-spectrum peak area, the molar ratio of compound A to compound B in composition 1# is calculated to be 2:1. Converted to mass ratio, compound A accounts for 78.4 wt% and compound B accounts for 21.6 wt%.
[0051] Example 2
[0052] The operation of this embodiment is the same as that of Embodiment 1, except that: the amount of boron trifluoride gas introduced in step S1 is increased to 0.20 mol, and the amount of lithium difluorophosphate added in step S2 is increased to 0.05 mol. The obtained additive composition is referred to as composition 2#.
[0053] NMR analysis showed that the nuclear magnetic resonance... 19 F-spectroscopy results showed no boron trifluoride residue in composition 2#. NMR spectroscopy... 19 Integrating the F-spectrum peak area, the molar ratio of compound A to compound B in composition 2# is calculated to be 1:1. Converted to mass percentage, compound A accounts for 64.5 wt% and compound B accounts for 35.5 wt%.
[0054] Example 3
[0055] The operation of this embodiment is the same as that of Embodiment 1, except that: the amount of boron trifluoride gas introduced in step S1 is increased to 0.25 mol, and the amount of lithium difluorophosphate added in step S2 is increased to 0.10 mol. The obtained additive composition is referred to as composition 3#.
[0056] NMR analysis showed that the nuclear magnetic resonance... 19 F-spectroscopy results showed no boron trifluoride residue in composition 3#. NMR... 19 Integrating the F-spectrum peak area, the molar ratio of compound A to compound B in composition 3# was calculated to be 1:2. Converted to mass percentage, compound A accounts for 47.6 wt% and compound B accounts for 52.4 wt%.
[0057] Example 4
[0058] The operation of this embodiment is the same as that of embodiment 1, except that: the amount of boron trifluoride gas introduced in step S1 is increased to 0.30 mol, and the amount of lithium difluorophosphate added in step S2 is increased to 0.15 mol. The obtained additive composition is referred to as composition 4#.
[0059] NMR analysis showed that the nuclear magnetic resonance... 19 F-spectroscopy results showed no boron trifluoride residue in composition 4#. NMR... 19 Integrating the F-spectrum peak area, the molar ratio of compound A to compound B in composition 4# was calculated to be 1:3. Converted to mass percentage, compound A accounts for 37.7 wt% and compound B accounts for 62.3 wt%.
[0060] Comparative Example 1
[0061] The operation of this comparative example is the same as that of Example 1, except that after obtaining the intermediate solution in step S1, step S2 is not performed. Instead, rotary evaporation is performed directly to obtain lithium tri(boron trifluoride) phosphate, denoted as compound A1.
[0062] NMR analysis showed that the nuclear magnetic resonance... 19 The F spectrum is shown below:
[0063] Compound A: δ = -157.48 ppm(s)
[0064] Boron trifluoride: δ = -152.71 ppm(s)
[0065] The results showed that boron trifluoride residues were present in compound A1. NMR spectroscopy... 19 Integrating the area of the F-spectrum peak, the molar ratio of boron trifluoride residue to compound A was calculated to be 0.5:1. Converted to mass percentage, compound A accounts for 90.42 wt%, and boron trifluoride accounts for 9.58 wt%.
[0066] Comparative Example 2
[0067] The operation of this comparative example is the same as that of Example 2, except that: after obtaining the intermediate solution in step S1, step S2 is not performed, but rotary evaporation is performed directly to obtain lithium tri(boron trifluoride) phosphate, denoted as compound A2.
[0068] NMR analysis showed that the nuclear magnetic resonance... 19 F-spectral results indicate the presence of boron trifluoride residue in compound A2. NMR spectroscopy... 19 Integrating the area of the F-spectrum peak, the molar ratio of boron trifluoride residue to compound A was calculated to be 0.5:1. Converted to mass percentage, compound A accounts for 90.42 wt%, and boron trifluoride accounts for 9.58 wt%.
[0069] Comparative Example 3
[0070] The operation in this embodiment is the same as in Embodiment 2, except that the amount of lithium difluorophosphate added in step S2 is reduced to 0.025 mol, and the obtained additive composition is designated as Composition 5#. Calculations show that the molar ratio between compound A, compound B, and residual boron trifluoride is 2:1:2, which translates to a mass percentage of 72.4 wt% for compound A, 20.0 wt% for compound B, and 7.60 wt% for boron trifluoride.
[0071] Comparative Example 4
[0072] The operation in this embodiment is the same as in Embodiment 3, except that the amount of lithium difluorophosphate added in step S2 is reduced to 0.05 mol, and the obtained additive composition is designated as Composition 6#. Calculations show that the molar ratio between compound A, compound B, and residual boron trifluoride is 1:1:1, which translates to a mass percentage of 56.8 wt% for compound A, 36.2 wt% for compound B, and 12.0 wt% for boron trifluoride.
[0073] By comparing the above examples and comparative examples, it can be found that the traditional rotary evaporation method cannot completely remove residual boron trifluoride from the product. Comparing Comparative Example 1 and Comparative Example 2, it can be seen that although the theoretical residual amounts of boron trifluoride in compounds A1 and A2 are different before rotary evaporation, the amount of boron trifluoride removed after rotary evaporation is limited, and the residual amount of boron trifluoride in compound A is ultimately between 9.5% and 10.0 wt%. However, by adding lithium difluorophosphate during the preparation process, the residual boron trifluoride can be completely removed and converted into compound B. Furthermore, the optimal addition amount of lithium difluorophosphate should conform to: molar amount of boron trifluoride added - molar amount of lithium phosphate added × 3. When the amount of lithium difluorophosphate added is low, boron trifluoride cannot be completely removed. When the content of lithium difluorophosphate is high, lithium difluorophosphate will remain in the additive composition, which is also applicable to electrolyte formulations that require the use of lithium difluorophosphate.
[0074] II. Application Examples
[0075] Preparation of basic electrolyte: In an argon-filled glove box (moisture < 5 ppm, oxygen < 10 ppm), ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were uniformly mixed at a mass ratio of EC:EMC:DEC = 3:5:2. LiPF6 was slowly added to the mixed solution until the mass fraction of LiPF6 reached 12.5%, thus obtaining the basic electrolyte.
[0076] Application Example 1
[0077] Add 1.0 wt% of composition 1# to the base electrolyte so that compound A accounts for 0.8% of the total mass of the electrolyte and compound B accounts for 0.2% of the total mass of the electrolyte.
[0078] Application Example 2
[0079] Add 1.2 wt% of composition 1# to the base electrolyte so that compound A accounts for 1.0% of the total mass of the electrolyte and compound B accounts for 0.2% of the total mass of the electrolyte.
[0080] Application Example 3
[0081] Add 2.0 wt% of composition 1# to the base electrolyte so that compound A accounts for 1.6% of the total mass of the electrolyte and compound B accounts for 0.4% of the total mass of the electrolyte.
[0082] Application Example 4
[0083] Add 2.0 wt% of composition 2# to the base electrolyte so that compound A accounts for 1.3% of the total mass of the electrolyte and compound B accounts for 0.7% of the total mass of the electrolyte.
[0084] Application Example 5
[0085] Add 2.0 wt% of composition 3# to the base electrolyte so that compound A accounts for 1.0% of the total mass of the electrolyte and compound B accounts for 1.0% of the total mass of the electrolyte.
[0086] Application Example 6
[0087] Add 2.0 wt% of composition 4# to the base electrolyte so that compound A accounts for 0.8% of the total mass of the electrolyte and compound B accounts for 1.2% of the total mass of the electrolyte.
[0088] Application Example 7
[0089] Add 4.2 wt% of composition 3# to the base electrolyte so that compound A accounts for 2.0% of the total mass of the electrolyte and compound B accounts for 2.2% of the total mass of the electrolyte.
[0090] Application Example 8
[0091] Add 7.0 wt% of composition 3# to the base electrolyte so that compound A accounts for 3.3% of the total mass of the electrolyte and compound B accounts for 3.7% of the total mass of the electrolyte.
[0092] Application Example 9
[0093] Add 2.0 wt% of composition 2# to the base electrolyte, so that compound A accounts for 1.3% of the total mass of the electrolyte and compound B accounts for 0.7% of the total mass of the electrolyte. At the same time, add 1% of vinylene carbonate (VC) of the total mass of the electrolyte.
[0094] Application Example 10
[0095] Add 2.0 wt% of composition 2# to the base electrolyte, so that compound A accounts for 1.3% of the total mass of the electrolyte and compound B accounts for 0.7% of the total mass of the electrolyte. At the same time, add 1% of 1,3-propanesulfonate lactone (PS) according to the total mass of the electrolyte.
[0096] Application Comparative Example 1
[0097] 2 wt% of compound A1 was added to the base electrolyte, wherein residual boron trifluoride (BF3) accounted for 0.2% of the total mass of the electrolyte.
[0098] Application Comparative Example 2
[0099] Add 2 wt% of compound B to the base electrolyte.
[0100] Application Comparative Example 3
[0101] The operation of this comparative example is the same as that of Example 5, except that boron trifluoride, accounting for 0.2% of the total mass of the electrolyte, is added.
[0102] Application Comparative Example 4
[0103] Add 2.2 wt% of composition 5# to the base electrolyte so that compound A accounts for 1.6% of the total mass of the electrolyte, compound B accounts for 0.4% of the total mass of the electrolyte, and residual boron trifluoride accounts for 0.2% of the total mass of the electrolyte.
[0104] Application Comparative Example 5
[0105] Add 2.3 wt% of composition 6# to the base electrolyte so that compound A accounts for 1.3% of the total mass of the electrolyte, compound B accounts for 0.7% of the total mass of the electrolyte, and residual boron trifluoride accounts for 0.3% of the total mass of the electrolyte.
[0106] III. Electrochemical Performance Testing
[0107] The electrolytes from the above embodiments and comparative examples were used to fabricate 1260mAh capacity soft-pack lithium-ion batteries. Each lithium-ion battery includes a positive electrode, a negative electrode, a separator, an electrolyte, and battery auxiliary materials. The positive electrode active material is a nickel-cobalt-manganese ternary material, and the negative electrode active material is a graphite-silicon mixture. The preparation process is as follows: the positive electrode, separator, and negative electrode are wound together into a core, sealed with an aluminum-plastic film, and then baked to ensure the electrode moisture content meets requirements. After baking, the battery cell is injected with electrolyte, and after standing, formation, capacity testing, and aging processes, the finished soft-pack battery cell is obtained.
[0108] The prepared lithium-ion power battery (soft-pack cell) was subjected to performance testing. The specific test items and methods are as follows:
[0109] (1) 60℃ high temperature storage test: Charge the battery to 100% SOC and store it in an oven at 60±2℃ for 28 days. Test the volume before and after storage to obtain the volume expansion rate of the single cell before and after storage at 60℃; test the DCR value after storage at room temperature and calculate the percentage value of the initial DCR, which is recorded as the discharge DCR change rate.
[0110] (2) 25℃ ambient temperature cycling test: The battery is cycled in an oven at 25±1℃ with a charge / discharge current of 1C / 1C. The discharge capacity is calculated every week. The cycle is stopped after 500 cycles, and the capacity retention rate is calculated after the cycle.
[0111] (3) -20℃ low temperature discharge: The battery is discharged to 80% of the lower limit voltage at a discharge current of 1C in an oven at -20±1℃. This is taken as the low temperature discharge capacity, and its percentage with the 1C discharge capacity at 25℃ is calculated and recorded as the low temperature discharge capacity retention rate.
[0112] The test results are shown in Table 1 below:
[0113] Table 1 Electrochemical performance test results
[0114]
[0115]
[0116] As shown in Table 1 above, adding a composition containing both compound A and compound B to the electrolyte can reduce the initial impedance of the battery, improve low-temperature discharge performance, suppress gas generation during high-temperature storage, and improve cycle performance, thus achieving a balance between high and low temperature performance. Comparing application examples 3-6 with comparative examples 2, 1, and 3 reveals that compounds A and B have a synergistic effect; compared to using either compound alone, their combined use achieves a balance between high and low temperature battery performance.
[0117] Comparing Application Examples 3-6 reveals that as the content of compound A in the composition gradually increases, the initial impedance and low-temperature discharge performance of the battery further improve. Conversely, as the content of compound B in the composition gradually increases, the high-temperature storage and cycle performance of the battery further improve. Comparing Application Examples 1 and 3, and Application Examples 5, 7, and 8 reveals that as the amount of composition added (the total amount of compound A and compound B) increases, the battery performance first improves and then deteriorates, with the optimal addition amount being around 2 wt%. Comparing Application Example 5 and Comparative Example 3, Application Example 3 and Comparative Example 4, and Application Example 4 and Comparative Example 5 reveals that the presence of boron trifluoride residue in the electrolyte worsens the battery's initial impedance, high-temperature storage, cycle performance, and low-temperature performance.
Claims
1. A method for preparing an electrolyte additive composition comprising lithium tri(boron trifluoride)phosphate and lithium (difluorophosphoryloxy)trifluoroborate, characterized in that: The preparation method includes: (1) Lithium phosphate and boron trifluoride gas or boron trifluoride complex react in the presence of a reaction solvent to obtain an intermediate solution, or lithium phosphate and boron trifluoride complex react to obtain an intermediate solution; the molar ratio of boron trifluoride to lithium phosphate is (3.5~6.0):1; the reaction temperature is 5~90℃, and the reaction time is 0.2~24h; (2) Lithium difluorophosphate is added to the intermediate solution and reacted at 5–90°C for 0.2–24 h to obtain a composition of lithium tri(boron trifluoride) phosphate as shown in formula (A) and lithium (difluorophosphoryloxy)trifluoroborate as shown in formula (B): The molar ratio of lithium difluorophosphate to lithium phosphate is (0.5–3.0):1; In the composition, the molar ratio of lithium tri(boron trifluoride)phosphate and lithium (difluorophosphoryloxy)trifluoroborate is between 2 / 1 and 1 / 3; no boron trifluoride residue remains.
2. The method for preparing the electrolyte additive composition according to claim 1, characterized in that: The boron trifluoride complex is selected from at least one of the following: boron trifluoride dimethyl carbonate complex, boron trifluoride diethyl ether complex, boron trifluoride dimethyl ether complex, boron trifluoride butyl ether complex, boron trifluoride ethyl acetate complex, boron trifluoride sulfolane complex, and boron trifluoride tetrahydrofuran complex.
3. The method for preparing the electrolyte additive composition according to claim 1, characterized in that: The reaction solvent is selected from at least one of dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, acetonitrile, or diethyl ether.
4. The method for preparing the electrolyte additive composition according to claim 3, characterized in that: The reaction solvent is selected from at least one of dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate.
5. A lithium-ion battery electrolyte, comprising a main lithium salt and a non-aqueous solvent, characterized in that: The electrolyte also contains an additive composition comprising lithium tri(boron trifluoride)phosphate and lithium (difluorophosphoryloxy)trifluoroborate, prepared by any of the preparation methods described in claims 1-4.
6. The lithium-ion battery electrolyte according to claim 5, characterized in that: Lithium tri(boron trifluoride) phosphate accounts for 0.01% to 10% of the total mass of the electrolyte, and lithium (difluorophosphoryloxy)trifluoroborate accounts for 0.01% to 10% of the total mass of the electrolyte, with the mass ratio of lithium tri(boron trifluoride) phosphate to lithium (difluorophosphoryloxy)trifluoroborate being (3.64 to 0.61):
1.
7. The lithium-ion battery electrolyte according to claim 6, characterized in that: Lithium tri(boron trifluoride) phosphate accounts for 0.2% to 5.0% of the total mass of the electrolyte, and lithium (difluorophosphoryloxy)trifluoroborate accounts for 0.2% to 5.0% of the total mass of the electrolyte.
8. The lithium-ion battery electrolyte according to claim 5, characterized in that: The main lithium salt is selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethylsulfonyl)imide, and its molar concentration is 0.1 to 4.0 mol / L.
9. The lithium-ion battery electrolyte according to claim 5, characterized in that: The non-aqueous solvent is selected from at least one of C3-C6 carbonate compounds, C3-C8 carboxylic acid ester compounds, sulfone compounds, and ether compounds.
10. The lithium-ion battery electrolyte according to any one of claims 5-9, characterized in that: The electrolyte further includes at least one of the following: vinylene carbonate, 1,3-propanesulfonate lactone, vinyl sulfate, 4-methyl vinyl sulfate, 4,4'-divinyl sulfate, fluoroethyl carbonate, difluoroethylene carbonate, tris(trimethylsilane) phosphate, tris(trimethylsilane) borate, lithium difluorophosphate, lithium difluorosulfonylimide, lithium difluorobis(oxalate) phosphate, and lithium difluorooxalate borate, with any one of them added accounting for 0.1% to 5.0% of the total mass of the electrolyte.
11. A lithium-ion battery, comprising a positive electrode, a negative electrode, and a separator, characterized in that: The lithium-ion battery further includes the electrolyte as described in claims 5-10.
Citation Information
Patent Citations
Nonaqueous electrolyte solution for batteries, novel compound, polymer electrolyte, and lithium secondary battery
CN105103361A
Nonaqueous electrolytic solution and lithium secondary battery
KR1020180050780A