Phosphomolybdic acid-mil-101 composite material, preparation method thereof and oil treatment method

By introducing phosphomolybdic acid into the in-situ synthesis of MIL-101 and treating it with NH₄F, a phosphomolybdic acid-MIL-101 composite material was prepared, which solved the problem of insufficient denitrification capacity and adsorption capacity in the existing technology and achieved efficient and economical fuel denitrification effect.

CN117942918BActive Publication Date: 2026-11-20CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211338704.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-28
Publication Date
2026-11-20
Estimated Expiration
2042-10-28

AI Technical Summary

Technical Problem

Existing technologies struggle to produce metal framework materials with good denitrification capabilities and high oil adsorption denitrification capacity. Furthermore, deep hydrodenitrification technology consumes a large amount of hydrogen and requires significant equipment investment, failing to meet the stringent requirements of environmental regulations.

Method used

By introducing phosphomolybdic acid into the in-situ synthesis of MIL-101 and improving the framework material with NH₄F, a phosphomolybdic acid-MIL-101 composite material was prepared. The synergistic effect of phosphomolybdic acid and MIL-101 was utilized to improve the denitrification capacity and adsorption denitrification capacity.

Benefits of technology

It significantly improves the denitrification rate and nitrogen adsorption capacity of oil products, has good material stability, is easy to recycle and regenerate, and is suitable for efficient adsorption and denitrification reactions of fuel under mild conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117942918B_ABST
    Figure CN117942918B_ABST
Patent Text Reader

Abstract

The application relates to a phosphomolybdic acid-MIL-101 composite material and a preparation method and an oil product treatment method. The preparation method comprises the following steps: (1) providing a first mixture comprising a MIL-101 starting raw material mixture and phosphomolybdic acid, then performing hydrothermal synthesis and separating an intermediate solid phase product; (2) mixing the intermediate solid phase product obtained in step (1), NH4F and water, and then separating a solid phase product. The phosphomolybdic acid-MIL-101 composite material comprises a MIL-101 base material and phosphomolybdic acid which is compounded in the MIL-101 base material, wherein at least part of the phosphomolybdic acid is distributed inside the pore channel of the MIL-101 base material. In the process of in-situ preparation of the MIL-101, the phosphomolybdic acid is directly introduced, then NH4F is used for optimization treatment, the prepared phosphomolybdic acid-MIL-101 composite material has better synergistic effect of the phosphomolybdic acid and the MIL-101, and the denitrification rate and the adsorbed nitrogen capacity of the oil product are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of MOF materials technology, specifically to a phosphomolybdic acid-MIL-101 composite material and its preparation method, as well as a method for treating oil products. Background Technology

[0002] When nitrogen-containing compounds in fuel burn in an engine, they react with O2 in the air to produce various nitrogen oxides (NOx) depending on the type of fuel and the degree of combustion. x NO x The generation of nitrogen oxides leads to numerous environmental pollution problems, such as acid rain and photochemical smog, which have a detrimental impact on public health and the balance of the ecological environment. With increasingly stringent environmental regulations, the production of ultra-low sulfur and low nitrogen "clean fuels" is receiving increasing attention worldwide, and the search for efficient, energy-saving, and environmentally friendly denitrification technologies has become a growing focus. Currently, diesel denitrification mainly includes hydrodenitrification and non-hydrodenitrification processes. Deep hydrodenitrification technology consumes a large amount of hydrogen, requires significant equipment investment, and is costly. As people's requirements for fuel cleanliness continue to increase, denitrification processes are increasingly developing towards economical, green, and environmentally friendly directions, making the development of new, environmentally friendly, and economical non-hydrodenitrification technologies essential. Non-hydrodenitrification processes include adsorption denitrification, solvent extraction, acid refining, complexation denitrification, microwave denitrification, biological denitrification, and oxidative extraction, among which adsorption denitrification is the most widely used. Compared with industrial hydrodenitrification processes, adsorption denitrification technology overcomes the disadvantage of decreased octane number and also solves the problems of high equipment investment and operating costs. Due to the advantages of adsorption denitrification and its potential application prospects, adsorption denitrification technology has become one of the key technologies developed by oil companies at home and abroad in recent years.

[0003] How to prepare a metal skeleton material with good denitrification ability and high oil adsorption denitrification capacity is a technical problem that urgently needs to be solved. Summary of the Invention

[0004] This invention provides a phosphomolybdic acid-MIL-101 composite material and its preparation method, as well as a method for treating oil products. By introducing phosphomolybdic acid during the in-situ preparation of MIL-101 and improving the skeleton material with NH4F, a phosphomolybdic acid-MIL-101 composite material with good denitrification ability and high oil adsorption denitrification capacity is obtained.

[0005] In a first aspect, the present invention relates to a method for preparing a phosphomolybdic acid-MIL-101 composite material, the method comprising the following steps: (1) providing a first mixture comprising a MIL-101 starting material mixture and phosphomolybdic acid, and then performing hydrothermal synthesis and separating an intermediate solid product; (2) mixing the intermediate solid product obtained from step (1), NH4F and water, and then separating the solid product.

[0006] Optionally, the MIL-101 starting material mixture includes chromium nitrate, terephthalic acid, a monobasic acid, and water.

[0007] Optionally, the monocarboxylic acid is selected from HF or HNO3.

[0008] Optionally, in the MIL-101 starting material mixture, the molar ratio of chromium nitrate, terephthalic acid, the monobasic acid, and water is 1:1:(0.4-1):(250-300).

[0009] Optionally, the chromium nitrate is Cr(NO3)3·9H2O, and the mass ratio of phosphomolybdic acid to the total mass of Cr(NO3)3·9H2O and terephthalic acid is (2-47):100; preferably, the mass ratio of phosphomolybdic acid to the total mass of Cr(NO3)3·9H2O and terephthalic acid is (2-20):100.

[0010] Optionally, in step (1), the hydrothermal synthesis temperature is 210-220℃ and the time is 7-10h.

[0011] Optionally, in step (2), the mass ratio of the intermediate solid product to NH4F is 1:(0.8-1.5), and the ratio of NH4F to water is 10mg:(0.5-1.5)ml.

[0012] Optionally, in step (2), the mixing temperature is 55-65℃; in step (2), the mixing is stirring, the stirring speed is 350-650 rpm, and the time is 8-12h.

[0013] In a second aspect, the present invention relates to a phosphomolybdic acid-MIL-101 composite material prepared according to the preparation method, the phosphomolybdic acid-MIL-101 composite material comprising a MIL-101 substrate and phosphomolybdic acid composited in the MIL-101 substrate, wherein at least a portion of the phosphomolybdic acid is distributed within the pores of the MIL-101 substrate.

[0014] Thirdly, the present invention relates to a method for processing oil products, wherein a phosphomolybdic acid-MIL-101 composite material is dispersed in the oil product, wherein the phosphomolybdic acid-MIL-101 composite material is prepared by the aforementioned preparation method or is the phosphomolybdic acid-MIL-101 composite material; preferably, the mass ratio of the phosphomolybdic acid-MIL-101 composite material to the oil product is (1-5):1000; more preferably, the oil product contains 200-500 ppm indole and / or 200-500 ppm quinoline.

[0015] Beneficial effects:

[0016] In the in-situ preparation of MIL-101, phosphomolybdic acid is directly introduced and then optimized with NH4F. The resulting phosphomolybdic acid-MIL-101 composite material exhibits better synergistic effects between phosphomolybdic acid and MIL-101, significantly improving the denitrification rate and nitrogen adsorption capacity of oil products. Attached Figure Description

[0017] Figure 1 This is a line graph showing the denitrification rate of the materials tested in Example 1;

[0018] Figure 2 This is a line graph showing the denitrification rate of the materials tested in Example 2;

[0019] Figure 3 This is a line graph showing the denitrification rate of the materials tested in Example 3;

[0020] Figure 4 This is the X-ray diffraction pattern of the corresponding material obtained by XRD testing in Example 5;

[0021] Figure 5 and 6 This is a SEM image of MIL-101NH4F prepared in Comparative Example 2;

[0022] Figure 7 and 8 This is a SEM image of PMA-MIL-101 (5% PMA, F / Cr = 1)NH4F prepared in Example 2;

[0023] Figure 9-1 Images 9 to 5 are TEM images and TEM elemental distribution maps of MIL-101 (F / Cr=1) prepared in Comparative Example 1;

[0024] Figures 10-1 to 10-7 The images show TEM images and TEM elemental distribution maps of PMA-MIL-101 (5% PMA, F / Cr=1) prepared in Comparative Example 4.

[0025] Figures 11-1 to 11-5 The images show TEM images and TEM elemental distribution diagrams of MIL-101NH4F (F / Cr=1) prepared in Comparative Example 2.

[0026] Figures 12-1 to 12-7 These are TEM images and TEM elemental distribution maps of PMA-MIL-101 (2% PMA, F / Cr = 1)NH4F prepared in Example 1;

[0027] Figures 13-1 to 13-7 These are TEM images and TEM elemental distribution maps of PMA-MIL-101 (5% PMA, F / Cr = 1)NH4F prepared in Example 2;

[0028] Figures 14-1 to 14-7 These are TEM images and TEM elemental distribution maps of PMA-MIL-101 (10% PMA, F / Cr=1)NH4F prepared in Example 3;

[0029] Figures 15-1 to 15-7 These are TEM images and TEM elemental distribution maps of PMA-MIL-101 (20% PMA, F / Cr = 1)NH4F prepared in Example 4;

[0030] Figure 16 This is the infrared spectrum obtained from test example 8;

[0031] Figure 17 and 18 These are the N2 adsorption-desorption curves and pore size diagrams obtained from test example 9;

[0032] Figure 19 This is the thermogravimetric curve obtained from test example 10. Detailed Implementation

[0033] The present application will now be described in further detail with reference to the accompanying drawings and embodiments. Through these descriptions, the features and advantages of the present application will become clearer and more apparent.

[0034] The term “exemplary” as used herein means “serving as an example, embodiment, or illustration.” Any embodiment illustrated herein as “exemplary” is not necessarily to be construed as superior to or better than other embodiments. Although various aspects of embodiments are shown in the accompanying drawings, the drawings are not necessarily drawn to scale unless specifically indicated otherwise.

[0035] Furthermore, the technical features involved in the different embodiments of this application described below can be combined with each other as long as they do not conflict with each other.

[0036] In a first aspect, the present invention relates to a method for preparing a phosphomolybdic acid-MIL-101 composite material, the method comprising the following steps:

[0037] (1) Provide a first mixture comprising a starting material mixture of MIL-101 and phosphomolybdic acid, then perform hydrothermal synthesis and separate the intermediate solid product; (2) Mix the intermediate solid product obtained from step (1), NH4F and water, and then separate the solid product.

[0038] It should be noted that in the preparation method of the present invention, phosphomolybdic acid, a specific substance, is introduced into the in-situ preparation of MIL-101 in step (1) and synthesized together with the starting material of MIL-101. This results in an intermediate solid phase product in which phosphomolybdic acid is distributed in the pores and on the surface of MIL-101. In step (2), the intermediate solid phase product is dispersed and mixed with NH4F in water. Firstly, NH4F removes almost all of the phosphomolybdic acid from the surface of MIL-101, leaving some phosphomolybdic acid in the pores of MIL-101. Secondly, the NH4F treatment in step (2) can largely eliminate the free carboxylic acid inside and outside the pores of MIL-101 and introduce more fluoride ions, allowing the pores in the resulting composite material to be utilized more fully. Thirdly, NH4F can remove the unstable framework in MIL-101, so that... The formation of more unsaturated metal active sites enables more effective adsorption and removal of nitrogen-containing compounds in fuel oil; fourth, some of the phosphomolybdic acid in the intermediate solid product obtained in step (1) is located in the pores of MIL-101. After the ammonium fluoride treatment in step (2), the phosphomolybdic acid in the pores is partially removed. Therefore, this process can greatly increase the pore volume of MIL-101, expose more unsaturated metal active sites, provide more open adsorption reaction sites for the reactants, and enable the composite material to more effectively adsorb and remove nitrogen-containing compounds in fuel oil.

[0039] In summary, this invention selects phosphomolybdic acid and MIL-101 as starting materials to synthesize a composite material of phosphomolybdic acid and MIL-101 in situ, and then performs NH4F treatment in step (2). In the phosphomolybdic acid-MIL-101 composite material obtained at this time, phosphomolybdic acid and MIL-101 can better exert synergistic effects, and the various synergistic effects of NH4F treatment are further enhanced. Therefore, the denitrification efficiency of the obtained composite material is significantly improved.

[0040] According to one embodiment of the first aspect of the present invention, the MIL-101 starting material mixture comprises chromium nitrate, terephthalic acid, a monobasic acid, and water.

[0041] It should be noted that in step (1), the first mixture composed of the several starting materials and phosphomolybdic acid can be dispersed in a hydrothermal reactor and placed in an oven, and then heated to carry out a hydrothermal reaction; specifically, chromium nitrate, terephthalic acid and phosphomolybdic acid can be dispersed and mixed in water first, and then a monobasic acid can be added, and then hydrothermal synthesis can be carried out.

[0042] According to one embodiment of the first aspect of the present invention, the monocarboxylic acid is selected from HF or HNO3.

[0043] It should be noted that in the preparation method of the present invention, in step (1), HF or HNO3 is used as a monobasic acid to carry out the hydrothermal synthesis in step (1), which can make the final phosphomolybdic acid-MIL-101 composite material have good denitrification performance.

[0044] According to one embodiment of the first aspect of the present invention, in the MIL-101 starting material mixture, the molar ratio of chromium nitrate, terephthalic acid, the monobasic acid and water can be 1:1:(0.4-1):(250-300).

[0045] It should be noted that several MIL-101 starting materials within the range of the stated molar ratio can react well to form MIL-101, wherein the molar ratio of F (or nitrate) to Cr can also be 0.7, preferably 1.

[0046] According to one embodiment of the first aspect of the present invention, the chromium nitrate is Cr(NO3)3·9H2O, and the mass ratio of phosphomolybdic acid to the total mass of Cr(NO3)3·9H2O and terephthalic acid can be (2-47):100; preferably, the mass ratio of phosphomolybdic acid to the total mass of Cr(NO3)3·9H2O and terephthalic acid is (2-20):100.

[0047] It should be noted that in the preparation method of the present invention, in the in-situ synthesis of MIL-101 by introducing phosphomolybdic acid in step (1), the mass ratio of the total mass of Cr(NO3)3·9H2O and terephthalic acid to the mass of phosphomolybdic acid must be within the range defined by the present invention to ensure that phosphomolybdic acid is introduced in a preferred content range. Therefore, the composite obtained in step (2) can maintain a preferred content of phosphomolybdic acid to achieve a good denitrification effect. As a preferred embodiment, the mass ratio of the total mass of Cr(NO3)3·9H2O and terephthalic acid to the mass of phosphomolybdic acid can be 5:1, 10:1, or 20:1. Alternatively, as a preferred embodiment, the mass of the added phosphomolybdic acid accounts for 2%, 5%, 10%, or 20% of the total mass of Cr(NO3)3·9H2O and terephthalic acid. By controlling the amount of phosphomolybdic acid to a preferred level, the performance of the prepared composite can be significantly improved, especially the total nitrogen adsorption capacity.

[0048] According to one embodiment of the first aspect of the present invention, in step (1), the temperature of the hydrothermal synthesis is 210-220°C and the time is 7-10h.

[0049] After the hydrothermal synthesis in step (1) is completed, the solid product can be separated by filtration and centrifugation. After separation, it can be washed and dried. Washing can be done with N,N-dimethylformamide (DMF). The solid powder obtained after washing and drying is the intermediate solid product. Specifically, the intermediate solid product obtained in step (1) can be centrifuged five times with dimethylformamide (DMF), and then mixed with NH4F as in step (2), such as stirring in an NH4F aqueous solution at 60°C for 10 hours. Then, it can be centrifuged three times with water at 60°C to obtain a pure composite material. The preparation method of the present invention greatly shortens the washing time, and the performance of the composite material obtained after simplification is significantly improved, such as the denitrification performance.

[0050] According to one embodiment of the first aspect of the present invention, in step (2), the mass ratio of the intermediate solid product to NH4F is 1:(0.8-1.5), and the ratio of NH4F to water is 10mg:(0.5-1.5)ml.

[0051] According to one embodiment of the first aspect of the present invention, in step (2), the mixing temperature is 55-65°C; in step (2), the mixing is a stirring mixing, the stirring speed is 350-650 rpm, and the time is 8-12 h.

[0052] It should be noted that the heating method in step (2) can be electric heating, water bath heating, oil bath heating, etc.; after mixing, separation and washing can be carried out, and separation can be carried out by centrifugation, filtration, etc.

[0053] In summary, the preparation method of this invention has simple equipment requirements, is easy to control, low in cost, and has good reproducibility, showing promise for large-scale production. In-situ PMA addition and NH4F solution treatment can significantly improve the adsorption and denitrification capacity of MIL-101 for oil products. Furthermore, the prepared material exhibits good stability, is easy to recycle, and can be used for efficient adsorption and denitrification reactions of fuel oil under mild conditions.

[0054] In a second aspect, the present invention relates to a phosphomolybdic acid-MIL-101 composite material prepared by the above preparation method, the phosphomolybdic acid-MIL-101 composite material comprising a MIL-101 substrate and phosphomolybdic acid composited in the MIL-101 substrate, wherein at least a portion of the phosphomolybdic acid is distributed inside the pores of the MIL-101 substrate.

[0055] It should be noted that, in this invention, MIL-101 refers to a MIL-101 type MOF material with Cr as the coordinating metal and terephthalic acid as the ligand. The phosphomolybdic acid-MIL-101 composite material described in this invention is a composite material containing both phosphomolybdic acid and MIL-101. Pmophosphomolybdic acid (PMA) can be represented as being loaded onto MIL-101, and some or all of the phosphomolybdic acid can be distributed in the pores of MIL-101.

[0056] It should be noted that the phosphomolybdic acid-MIL-101 composite material of the present invention combines the advantages of both materials. It possesses the high specific surface area of ​​MIL-101, providing open adsorption reaction sites for reactants, and also anchors the PMA active centers within the cavities of MIL-101 through a confinement effect, effectively removing aromatic nitrogen-containing compounds from fuel oil. Specifically, PMA can provide... The B acid (B acid) sites, MIL-101 can provide Lewis acid (L acid) sites, and the synergistic effect of B acid and L acid enables the composite material to effectively adsorb and remove nitrogen-containing compounds from fuel.

[0057] It should be noted that in the phosphomolybdic acid-MIL-101 composite material, phosphomolybdic acid may be partially located inside the pores of the MIL-101 substrate, or it may be entirely distributed inside the pores of the MIL-101 substrate.

[0058] Thirdly, the present invention relates to a method for processing oil products, wherein a phosphomolybdic acid-MIL-101 composite material is dispersed in the oil product, wherein the phosphomolybdic acid-MIL-101 composite material is the phosphomolybdic acid-MIL-101 composite material or is prepared by the preparation method described above; preferably, the mass ratio of the phosphomolybdic acid-MIL-101 composite material to the oil product is (1-5):1000; more preferably, the oil product contains 200-500 ppm indole and / or 200-500 ppm quinoline.

[0059] It should be noted that in the oil treatment method of the present invention, denitrification can be achieved by adding the adsorbent and stirring. The denitrification time can be 1 hour. Denitrification can be carried out at room temperature, and nitrogen-containing compounds can be removed well under mild conditions.

[0060] The present invention will be further described in detail below through examples, but these examples are not intended to limit the invention.

[0061] All reagents used in the following examples are commercially available finished reagents.

[0062] In the following examples, BDC represents terephthalic acid, PMA represents phosphomolybdic acid, and DMF represents N,N-dimethylformamide. See Table 1 below and... Figure 1 Table 2 and Figure 2 and Table 3 and Figure 3 In the table, the serial numbers correspond to the serial numbers on the horizontal axis of the graph, and F / Cr represents the molar ratio of F (HF) and Cr.

[0063] Example 1

[0064] Weigh 1.6g Cr(NO3)3·9H2O, 656mg BDC, and 2% PMA (the total mass of Cr(NO3)3·9H2O and BDC), disperse them in 19.2mL water, add 174ul HF solution (mass fraction 40%), sonicate for 5min, transfer the mixture to a reaction vessel, heat in a constant temperature oven at 220℃ for 8h, wash with DMF and collect the generated solid powder (e.g., centrifuge 5 times) to obtain PMA-MIL-101 (2% PMA).

[0065] Weigh 488 mg of PMA-MIL-101 (2% PMA) and 541.68 mg of NH4F and disperse them in 73.2 ml of water. Pour the solution into a 250 ml round-bottom flask, set the stirring speed to 500 rpm, and stir at 60 °C for 10 h. Wash with water and collect the resulting solid powder to obtain the NH4F-treated composite material product, which can be represented as PMA-MIL-101 (2% PMA, F / Cr = 1)NH4F.

[0066] Example 2

[0067] Weigh 1.6 g of Cr(NO3)3·9H2O, 656 mg of BDC, and 5% of the total mass of Cr(NO3)3·9H2O and BDC in PMA, disperse them in 19.2 mL of water, add 174 μL of HF solution (mass fraction 40%), sonicate for 5 min, transfer the mixture to a reaction vessel, heat it in a constant temperature oven at 220 °C for 8 h, wash with DMF and collect the resulting solid powder to obtain PMA-MIL-101 (5% PMA).

[0068] Weigh 488 mg of PMA-MIL-101 (5% PMA) and 541.68 mg of NH4F and disperse them in 73.2 ml of water. Pour the solution into a 250 ml round-bottom flask, set the stirring speed to 500 rpm, and stir at 60 °C for 10 h. Wash with water and collect the resulting solid powder to obtain the NH4F-treated composite material product, which can be represented as PMA-MIL-101 (5% PMA, F / Cr = 1)NH4F.

[0069] Example 3

[0070] Weigh 1.6 g of Cr(NO3)3·9H2O, 656 mg of BDC, and 10% of the total mass of Cr(NO3)3·9H2O and BDC in PMA, disperse them in 19.2 mL of water, add 174 μL of HF solution (mass fraction of 40%), sonicate for 5 min, transfer the mixture to a reaction vessel, heat it in a constant temperature oven at 220 °C for 8 h, wash with DMF and collect the resulting solid powder to obtain PMA-MIL-101 (10% PMA).

[0071] Weigh 488 mg of PMA-MIL-101 (10% PMA) and 541.68 mg of NH4F and disperse them in 73.2 ml of water. Pour the solution into a 250 ml round-bottom flask, set the stirring speed to 500 rpm, and stir at 60 °C for 10 h. Wash with water and collect the resulting solid powder to obtain the NH4F-treated composite material product, which can be represented as PMA-MIL-101(10% PMA, F / Cr=1)NH4F.

[0072] Example 4

[0073] Weigh 1.6 g of Cr(NO3)3·9H2O, 656 mg of BDC, and 20% of the total mass of Cr(NO3)3·9H2O and BDC in PMA, disperse them in 19.2 mL of water, add 174 μL of HF solution (mass fraction 40%), sonicate for 5 min, transfer the mixture to a reaction vessel, heat it in a constant temperature oven at 220 °C for 8 h, wash with DMF and collect the resulting solid powder to obtain PMA-MIL-101 (20% PMA).

[0074] Weigh 488 mg of PMA-MIL-101 (20% PMA) and 541.68 mg of NH4F and disperse them in 73.2 ml of water. Pour the solution into a 250 ml round-bottom flask, set the stirring speed to 500 rpm, and stir at 60 °C for 10 h. Wash with water and collect the resulting solid powder to obtain the NH4F-treated composite material product, which can be represented as PMA-MIL-101(20% PMA, F / Cr=1)NH4F.

[0075] Example 5

[0076] Weigh 1.6 g of Cr(NO3)3·9H2O, 656 mg of BDC, and 47% of the total mass of Cr(NO3)3·9H2O and BDC in PMA. Disperse the mixture in 19.2 mL of water, add 174 μL of HF solution (40% by mass), sonicate for 5 min, transfer the mixture to a reaction vessel, heat it in a constant temperature oven at 220 °C for 8 h, wash with DMF and collect the resulting solid powder to obtain PMA-MIL-101 (47% PMA).

[0077] Weigh 488 mg of PMA-MIL-101 (47% PMA) and 541.68 mg of NH4F and disperse them in 73.2 ml of water. Pour the solution into a 250 ml round-bottom flask, set the stirring speed to 500 rpm, and stir at 60 °C for 10 h. Wash with water and collect the resulting solid powder to obtain the NH4F-treated composite material product, which can be represented as PMA-MIL-101 (47% PMA, F / Cr = 1)NH4F.

[0078] Comparative Example 1

[0079] Preparation of MIL-101 material:

[0080] Weigh 1.6 g Cr(NO3)3·9H2O and 656 mg BDC, disperse them in 19.2 mL of water, and add 70 μL, 122 μL, and 174 μL of HF solution (40% by mass) respectively. Sonicate for 5 min, transfer the mixture to a reaction vessel, and heat in a constant temperature oven at 220 °C for 8 h. Wash with DMF and collect the resulting solid powder to prepare three types of MIL-101 with different F / Cr ratios:

[0081] MIL-101 (F / Cr=0.4), MIL-101 (F / Cr=0.7) and MIL-101 (F / Cr=1).

[0082] Following the method for preparing MIL-101 (F / Cr = 1), 174 μL of HF solution (40% by mass) was replaced with 257 μL of 68% nitric acid to prepare MIL-101 (NO3). - / Cr=1).

[0083] Comparative Example 2

[0084] Preparation of MIL-101NH4F material:

[0085] 488 mg of MIL-101 and 541.68 mg of NH4F prepared in Comparative Example 1 were dispersed in 73.2 ml of water. The solution was poured into a 250 ml round-bottom flask, stirred at 500 rpm and 60 °C for 10 h, and the resulting solid powder was collected after washing with water to prepare three types of MIL-101-NH4F with different F / Cr ratios:

[0086] MIL-101NH4F (F / Cr=0.4), MIL-101NH4F (F / Cr=0.7) and MIL-101NH4F (F / Cr=1).

[0087] Take 488 mg of MIL-101 (NO3) prepared in Comparative Example 1 - / Cr=1) and 541.68mg NH4F were dispersed in 73.2ml of water. The solution was poured into a 250ml round-bottom flask, stirred at 500rpm and 60℃ for 10h, and the resulting solid powder was collected after washing with water to obtain MIL-101 (NO3). - / Cr=1)NH4F.

[0088] Comparative Example 3

[0089] Preparation of PMA@MIL-101NH4F composite material:

[0090] Weigh 30 mg PMA and 300 mg MIL-101NH4F prepared in Comparative Example 2, disperse them in 60 mL of a mixed solution of ethanol and water (volume ratio 1:1), transfer the mixture to a reaction vessel, heat it in a constant temperature oven at 100 °C for 12 h, wash with water and ethanol to collect the resulting solid powder, and obtain three PMA@MIL-101-NH4F with different F / Cr ratios:

[0091] PMA@MIL-101NH4F (F / Cr=0.4), PMA@MIL-101NH4F (F / Cr=0.7) and PMA@MIL-101NH4F (F / Cr=1).

[0092] Based on MIL-101 (NO3) in Comparative Example 2 - PMA@MIL-101 (NO3) was prepared by reacting NH4F with Cr=1. - / Cr=1)NH4F.

[0093] Comparative Example 4

[0094] Preparation of PMA-MIL-101 composite material:

[0095] Weigh 1.6 g of Cr(NO3)3·9H2O, 656 mg of BDC, and PMA, disperse them in 19.2 mL of water, add 174 μL of HF solution (40% by mass), sonicate for 5 min, transfer the mixture to a reaction vessel, heat in a constant temperature oven at 220 °C for 8 h, and collect the resulting solid powder by washing with DMF. The added PMA masses were 2% of the total mass of Cr(NO3)3·9H2O and BDC, 5% of the total mass of Cr(NO3)3·9H2O and BDC, 10% of the total mass of Cr(NO3)3·9H2O and BDC, and 20% of the total mass of Cr(NO3)3·9H2O and BDC, respectively, to prepare four types of PMA-MIL-101 composite materials:

[0096] PMA-MIL-101 (2% PMA, F / Cr=1), PMA-MIL-101 (5% PMA, F / Cr=1), PMA-MIL-101 (10% PMA, F / Cr=1) and PMA-MIL-101 (20% PMA, F / Cr=1).

[0097] Comparative Example 5

[0098] Preparation of phosphotungstic acid (PTA)-MIL-101 composite material:

[0099] Weigh 4g Cr(NO3)3·9H2O, 1.66g BDC and 2.66g PTA (phosphotungstic acid), disperse them in 52mL water, add 450ul HF solution (mass fraction of 40%), sonicate for 5min, transfer the mixture to a reaction vessel, heat in a constant temperature oven at 220℃ for 8h, wash with DMF and collect the generated solid powder to obtain PTA-MIL-101 (47% PTA).

[0100] Weigh 488 mg PTA-MIL-101 (47% PTA) and 541.68 mg NH4F and disperse them in 73.2 ml of water. Pour the solution into a 250 ml round-bottom flask, set the stirring speed to 500 rpm, and stir at 60 °C for 10 h. Wash with water and collect the resulting solid powder to obtain the NH4F-treated composite material product, which can be represented as PTA-MIL-101 (47% PTA, F / Cr = 1)NH4F.

[0101] Test Example 1

[0102] An octane solution containing 200 ppm indole and 200 ppm quinoline was used as a nitrogen-containing simulated oil. Materials prepared in the above examples and comparative examples were used as adsorbents. 20 mg of adsorbent was added to 10 g of nitrogen-containing simulated oil, and the mixture was stirred at 500 rpm for 1 h at room temperature. The concentrations of indole and quinoline before and after adsorption were analyzed by liquid chromatography. The denitrification rate, adsorption nitrogen capacity, and total adsorption nitrogen capacity were then calculated. The results are shown in Table 1 below. A line graph showing the denitrification rate calculated based on the concentrations of indole and quinoline before and after adsorption is shown below. Figure 1 After denitrification, the mixture was centrifuged, and the supernatant was collected. The concentration of quinoline or indole was then analyzed by liquid chromatography.

[0103] Denitrification rate (%) = (Concentration of nitrogen compounds in nitrogen-containing simulated oil before adsorption - Concentration of nitrogen compounds in nitrogen-containing simulated oil after adsorption) ÷ Concentration of nitrogen compounds in nitrogen-containing simulated oil before adsorption × 100%.

[0104] Adsorption nitrogen capacity

[0105] Total adsorbed nitrogen capacity = q = q (喹啉) +q(吲哚) .

[0106] q represents the nitrogen adsorption capacity (i.e., the number of micrograms of nitrogen adsorbed per gram of adsorbent), m1 is the mass (g) of the adsorbed nitrogen-denitrifying model oil, and c o It is the mass concentration (ppm) of nitrides in the model oil before adsorption. e M1 is the mass concentration (ppm) of nitrides after the model oil is adsorbed, M2 is the mass (g) of the adsorbent, M1 is the molar mass of N, and M2 is the molar mass of nitrides.

[0107] Table 1

[0108]

[0109] In Table 1, the adsorbents for serial numbers 1-3 are MIL-101 (F / Cr = 0.4), MIL-101 (F / Cr = 0.7), and MIL-101 (F / Cr = 1) prepared in Comparative Example 1; the adsorbents for serial numbers 4-6 are MIL-101NH4F (F / Cr = 0.4), MIL-101NH4F (F / Cr = 0.7), and MIL-101NH4F (F / Cr = 1) prepared in Comparative Example 2; and the adsorbents for serial numbers 7-9 are PMA@MIL-101NH4F (F / Cr = 0.4), PMA@MIL-101NH4F (F / Cr = 0.7), and PMA@MIL-101NH4F (F / Cr = 1) prepared in Comparative Example 3.

[0110] From Table 1 and Figure 1 As can be seen, compared with the three different F / Cr molar ratios of MIL-101 synthesized in Comparative Example 1, the removal efficiency of the NH4F-treated MIL-101-NH4F material prepared in Comparative Example 2 and the PMA@MIL-101-NH4F material prepared in Comparative Example 3 for the basic nitrogen compound quinoline and the non-basic nitrogen compound indole was significantly improved. This is because the hydrothermal synthesized MIL-101 contains a large number of unformed carboxylic acids inside and outside the pores, which hides the metal active sites of MIL-101 and reduces the usable pore size. However, the specific surface area of ​​the MIL-101 material treated with NH4F is greatly increased, and more metal active sites are exposed, thus enabling the MIL-101 material to produce a significant adsorption and denitrification effect on simulated oil within 1 hour.

[0111] Test Example 2

[0112] The materials prepared in the above examples and comparative examples were tested and the denitrification rate, adsorption nitrogen capacity, and total adsorption nitrogen capacity were calculated according to the method of Test Example 1, with the following differences:

[0113] The added adsorbent mass was 30 mg, and the concentrations of indole and quinoline in the nitrogen-containing simulated oil were 500 ppm. The denitrification rate, adsorption nitrogen capacity, and total adsorption nitrogen capacity are shown in Table 2 below. A line graph showing the denitrification rate calculated using the indole and quinoline concentrations before and after the addition is shown below. Figure 2 .

[0114] Table 2

[0115]

[0116]

[0117] In Table 2, the adsorbent for serial number 1 is MIL-101 (F / Cr = 0.7) prepared in Comparative Example 1, and the adsorbents for serial numbers 2-4 and 8 are MIL-101NH4F (F / Cr = 0.4), MIL-101NH4F (F / Cr = 0.7), MIL-101NH4F (F / Cr = 1), and MIL-101(NO3) prepared in Comparative Example 2. - The adsorbents in items 5-7 are PMA@MIL-101NH4F (F / Cr=0.4), PMA@MIL-101NH4F (F / Cr=0.7) and PMA@MIL-101NH4F (F / Cr=1) prepared in Comparative Example 3, and the adsorbent in item 9 is PMA-MIL-101 (47% PMA, F / Cr=1)NH4F prepared in Example 5.

[0118] As can be seen from Table 2, compared with the MIL-101F / Cr=0.7 material prepared in Comparative Example 1, the removal efficiency of the NH4F-treated MIL-101 prepared in Comparative Example 2, the NH4F-treated PMA@MIL-101 prepared in Comparative Example 3, and the NH4F-treated PMA-MIL-101 material prepared in Example 5 for the removal of basic nitrogen compounds quinoline and non-basic nitrogen compounds indole were significantly improved. Among them, the denitrification efficiency of the PMA@MIL-101 composite material prepared by impregnation-loaded PMA in Comparative Example 3 after NH4F treatment was not much different from that of the pure MIL-101 prepared in Comparative Example 2 after NH4F treatment. However, the composite material PMA-MIL-101 (47% PMA, F / Cr=1) prepared in Example 5 showed the best overall performance in terms of denitrification rate and nitrogen adsorption capacity among these materials.

[0119] Subsequently, attempts were made to replace HF in the synthesized material with nitric acid (serial number 8) or to add PMA in situ (serial number 9), and the denitrification effect of the generated MIL-101 series materials was tested, resulting in more superior adsorption and denitrification activity.

[0120] In the examples, the denitrification effect of PMA-MIL-101 prepared by in-situ addition of PMA after NH4F treatment is better than that of MIL-101 prepared in the comparative example after NH4F treatment, and also better than PMA@MIL-101 prepared by impregnation method and treated with NH4F in the comparative example.

[0121] The advantage of in-situ PMA addition in this embodiment compared to the comparative impregnation method is that NH4F washes away excess PMA in the pores, generating more pores and exposing more metal active sites. In comparison, NH4F treatment remains the most significant method for improving the denitrification effect of MIL-101. Specifically, in this embodiment, the introduction of PMA during the in-situ preparation of MIL-101 followed by NH4F treatment significantly improves the denitrification effect of the prepared phosphomolybdic acid-MIL-101 composite material.

[0122] Test Example 3

[0123] The materials prepared in the above examples and comparative examples were tested and the denitrification rate, adsorption nitrogen capacity, and total adsorption nitrogen capacity were calculated according to the method of Test Example 1, with the following differences:

[0124] The added adsorbent mass was 20 mg, and the concentrations of indole and quinoline in the nitrogen-containing simulated oil were 500 ppm. The denitrification rate, adsorption nitrogen capacity, and total adsorption nitrogen capacity are shown in Table 3 below. A line graph showing the denitrification rate calculated using the indole and quinoline concentrations before and after the addition is shown below. Figure 3 .

[0125] Table 3

[0126]

[0127] In Table 3, the adsorbent for item 1 is MIL-101 (F / Cr = 1) prepared in Comparative Example 1; the adsorbents for items 2-5 are PMA-MIL-101 (2-20% PMA, F / Cr = 1) prepared in Comparative Example 4; the adsorbent for item 6 is MIL-101NH4F (F / Cr = 1) prepared in Comparative Example 2; and the adsorbents for items 7-10 are PMA-MIL-101 (2-20% PMA, F / Cr = 1)NH4F prepared in Examples 1-4. The adsorbent for item 11 is PTA-MIL-101 (47% PTA, F / Cr = 1)NH4F prepared in Comparative Example 5.

[0128] The F / Cr ratio in the materials tested in this embodiment was 1. (From Table 3 and...) Figure 3Points 2-5 and 7-11 show that the denitrification performance of the PTA-modified PTA-MIL-101 (47% PTA, F / Cr=1)NH4F composite material is inferior to that of the PMA-MIL-101 (2-20% PMA, F / Cr=1)NH4F composite material. However, compared with PMA-MIL-101 composite materials with different PMA contents, the removal efficiency of the NH4F-treated PMA-MIL-101 composite material for both basic nitrogen compounds (quinoline) and non-basic nitrogen compounds (indole) is significantly improved. The total nitrogen adsorption capacity of the PMA-MIL-101 composite material before and after NH4F treatment can differ by about 5-6 times. In summary, the composite material prepared by the method of this invention can maintain a stable structure of MIL-101 under NH4F treatment and greatly improve its denitrification effect. PMA and MIL-101NH4F play a synergistic role, greatly improving the denitrification performance of the material.

[0129] By comparing and analyzing the data in Table 3 (items 7-10) and Table 2 (item 9, PTA-MIL-101 (47% PMA, F / Cr=1)NH4F prepared in Example 5), it can be seen that the total adsorption nitrogen capacity of items 8-10 in Table 3 (PMA-MIL-101 (5%, 10%, and 20% PMA, F / Cr=1)NH4F) is significantly increased. This indicates that by specifically introducing phosphomolybdic acid as a heteropoly acid and controlling the amount of phosphomolybdic acid introduced, the total adsorption nitrogen capacity of the composite material can be significantly improved.

[0130] Test Example 4

[0131] ICP analysis was performed on the materials prepared in the above embodiments and comparative examples to detect the elemental content of F. The results are shown in Table 4 below:

[0132] Table 4

[0133]

[0134] In Table 4, MIL101 is MIL-101 (F / Cr=1) prepared in Comparative Example 1, MIL101 NH4F is MIL-101NH4F (F / Cr=1) prepared in Comparative Example 2, PMA-MIL101 5%PMA is PMA-MIL-101 (5%PMA, F / Cr=1) prepared in Comparative Example 4, and PMA-MIL101 5%PMA NH4F is PMA-MIL-101 (5%PMA, F / Cr=1)NH4F prepared in Example 2.

[0135] As shown in Table 4, the F content of MIL-101 prepared in Comparative Example 1 without NH4F treatment and PMA-MIL-101 prepared in Comparative Example 4 is only 0.075 wt.% and 0.128 wt.%, respectively. However, the F content of MIL-101NH4F prepared in Comparative Example 2 and PMA-MIL-101NH4F prepared in Example 2 after NH4F treatment increases to 1.853 wt.% and 1.482 wt.%, respectively. According to DFT (density functional theory) calculations, the more OH and H2O on the three Cr atoms in the Cr3(μ3-O)(F / OH)(H2O)2(C8H4O4)3 cluster of MIL-101 are replaced by F, the higher the adsorption energy for indole and quinoline increases. The increase in F content in MIL-101 greatly improves the adsorption and denitrification performance. As shown in Table 4, the F content in the composite material prepared in this application is significantly higher than that in the 5% PMA-MIL101 without NH4F treatment. This indicates that the in-situ preparation of the PMA and MIL-101 composite material followed by NH4F treatment allows for the introduction of a large amount of F into the MIL-101, greatly increasing the F element content and thus obtaining a PMA and MIL-101 composite material with significantly improved denitrification effect.

[0136] In addition, the content of Mo in the composite materials prepared in Examples 1-5 was detected by ICP analysis. Mo was detected in all the composite materials prepared in the examples, indicating that the preparation method of the present invention successfully introduced phosphomolybdic acid into MIL-101. Moreover, the Mo content in the PMA-MIL-101NH4F material prepared in the examples increased with the increase of PMA dosage.

[0137] Test Example 5

[0138] The materials prepared in the above embodiments and comparative examples were subjected to XRD analysis, and the obtained XRD diffraction patterns are shown in the figure. Figure 4 . Figure 4In the diagram, from top to bottom, the diffraction lines at positions 1-4 are the diffraction lines of the four composites prepared in Examples 4 to 1; the diffraction lines at positions 5-7 are the diffraction lines of PMA@MIL-101NH4F (F / Cr = 1), PMA@MIL-101NH4F (F / Cr = 0.7), and PMA@MIL-101NH4F (F / Cr = 0.4) prepared in Comparative Example 3; and the diffraction lines at positions 8-10 are the diffraction lines of MIL-1 prepared in Comparative Example 2. Diffraction lines of MIL-101NH4F (F / Cr = 1), MIL-101NH4F (F / Cr = 0.7), and MIL-101NH4F (F / Cr = 0.4) are shown. Diffraction lines at positions 11-13 are diffraction lines of MIL-101 (F / Cr = 1), MIL-101 (F / Cr = 0.7), and MIL-101 (F / Cr = 0.4) prepared in Comparative Example 1. "Simulate" refers to the diffraction lines of a commercially available MIL-101 standard. Figure 4 As can be seen from the XRD diffraction lines of the composite material prepared in the embodiments of this application, the characteristic peaks of MIL-101 material are clearly present, indicating that MIL-101 in the composite material prepared by the method of this invention maintains a good crystal form. Furthermore, the characteristic peaks of phosphomolybdic acid did not appear in the XRD diffraction lines of the composite material prepared in the above embodiments, and the ICP results indicate the presence of Mo, indicating that phosphomolybdic acid is distributed within the pores of MIL-101 in the composite material prepared in the embodiments.

[0139] Test Example 6

[0140] The materials prepared in the examples and comparative examples were analyzed by scanning electron microscopy, and the obtained SEM images are shown in the respective figures. Figure 5-8 . Figure 5-6 Here is an electron microscope image of MIL-101 NH4F prepared in Comparative Example 2. Figure 7-8 SEM image of PMA-MIL-101 (5% PMA, F / Cr = 1)NH4F prepared in Example 2. (The image is obtained through...) Figure 5-8 As can be seen, the composite material prepared by in-situ introduction of PMA in the embodiments of this application basically maintains a good morphology, and the elements are uniformly distributed in the material without agglomeration on the material surface. This indicates that PMA is well confined in the pores of MIL-101.

[0141] Test Example 7

[0142] The materials prepared in the examples and comparative examples were analyzed by transmission electron microscopy (TEM). The obtained TEM images and elemental distribution maps are shown in the figure. Figure 9-1 Up to 9-5, Figures 10-1 to 10-7 , Figures 11-1 to 11-5 , Figures 12-1 to 12-7 , Figures 13-1 to 13-7 , Figures 14-1 to 14-7 , Figures 15-1 to 15-7 .

[0143] Figure 9-1 Figures 9 to 5 represent the characterization results of the MIL-101 (F / Cr = 1) material prepared in Comparative Example 1. Figures 10-1 to 10-7 The characterization results are for PMA-MIL-101 (5% PMA, F / Cr = 1) prepared in Comparative Example 4; Figures 11-1 to 11-5 The characterization results are for MIL-101NH4F (F / Cr=1) prepared in Comparative Example 2; Figures 12-1 to 12-7 The characterization results are for PMA-MIL-101 (2% PMA, F / Cr = 1)NH4F prepared in Example 1; Figures 13-1 to 13-7 The characterization results are for PMA-MIL-101 (5% PMA, F / Cr = 1)NH4F prepared in Example 2; Figures 14-1 to 14-7 The characterization results are for PMA-MIL-101 (10% PMA, F / Cr = 1)NH4F prepared in Example 3; Figures 15-1 to 15-7 The characterization results are for PMA-MIL-101 (20% PMA, F / Cr = 1)NH4F prepared in Example 4.

[0144] The results obtained from TEM images and elemental distribution maps are consistent with those from SEM. The elements are uniformly distributed in the material and do not agglomerate on the material surface. Furthermore, the composite material containing PMA in the raw material has corresponding trace amounts of P and Mo. The composite material treated with NH4F also shows the same results. This indicates the presence of trace amounts of PMA and that it is well confined within the pores of MIL-101.

[0145] The elemental distribution diagrams obtained by transmission electron microscopy in Examples 1-4 show that the composite material was successfully obtained by combining phosphomolybdic acid and MIL-101 using the method of the present invention.

[0146] Test Example 8

[0147] Infrared analysis was performed on the materials prepared in the examples and comparative examples, and the resulting infrared spectra are shown below. Figure 16 .

[0148] exist Figure 16In this context, PMA is commercially available finished phosphomolybdic acid; PMA-MIL-101 NH4F 2% PMA to PMA-MIL-101 NH4F 20% PMA is the PMA-MIL-101 (2-20% PMA, F / Cr=1) NH4F prepared in Examples 1-4; MIL-101 NH4F is the MIL-101 NH4F (F / Cr=1) prepared in Comparative Example 2; PMA-MIL-101 2% to PMA-MIL-101 20% is the PMA-MIL-101 (2-20% PMA, F / Cr=1) prepared in Comparative Example 4; and MIL-101 is the MIL-101 (F / Cr=1) prepared in Comparative Example 1.

[0149] Figure 16 In Comparative Example 4, the infrared radiation of the four types of PMA-MIL-101 prepared at 959 cm⁻¹ was [not specified]. -1 The characteristic infrared absorption peak of PMA is located at position 959 cm⁻¹, indicating that PMA was successfully introduced into MIL-101 during the in-situ synthesis of PMA, as shown by the infrared spectrum. The infrared spectrum of the four complexes prepared in the examples is at 959 cm⁻¹. -1 The decrease in PMA intensity at the specified location indicates that a large amount of PMA was washed away after cleaning with NH4F solution, leaving only a small amount. Comparing PMA-MIL-101 before and after NH4F cleaning revealed that the characteristic PMA peak (959 cm⁻¹) at PMA-MIL-101 after NH4F cleaning was significantly reduced. -1 The intensity decreased (proven in conjunction with transmission mapping), demonstrating a reduction in PMA. After NH4F cleaning, the PMA was 1666 cm⁻¹. -1 and 1444cm -1 The disappearance of the free carboxylic acid peak indicates that the free carboxylic acid in the pores has been washed away, exposing the pores of MIL-101.

[0150] Test Example 9

[0151] The N2 adsorption-desorption tests were performed on the materials prepared in the examples and comparative examples. The obtained N2 adsorption-desorption curves and pore size diagrams are shown in the figures below. Figure 17 and Figure 18 The measured specific surface area and pore volume parameters are shown in Table 5 below.

[0152] Figure 17 , 18In Table 5, MIL-101 is the MIL-101 (F / Cr=1) prepared in Comparative Example 1, PMA-MIL-101 2% PMA to PMA-MIL-101 20% PMA are the PMA-MIL-101 (2% PMA, F / Cr=1) to PMA-MIL-101 (20% PMA, F / Cr=1) prepared in Comparative Example 4, MIL-101 NH4F is the MIL-101 NH4F (F / Cr=1) prepared in Comparative Example 2, and PMA-MIL-101 2% PMA NH4F to PMA-MIL101 20% PMA NH4F are the PMA-MIL-101 (2% PMA, F / Cr=1) NH4F to PMA-MIL-101 (20% PMA, F / Cr=1) NH4F prepared in Examples 1-4.

[0153] It can be seen that the specific surface area of ​​PMA-MIL-101 is relatively low compared to that of MIL-101 after synthesis. After cleaning with NH4F, its specific surface area and pore volume are greatly increased (Table 5). This proves that the in-situ addition of PMA and cleaning with NH4F can expand the micropore size and increase the specific surface area. This has a direct impact on the high oil denitrification performance of PMA-MIL-101 material.

[0154] Table 5

[0155]

[0156]

[0157] * indicates that it has not been tested.

[0158] Test Example 10

[0159] Thermogravimetric analysis was performed on the materials prepared in the above embodiments and comparative examples, and the obtained thermogravimetric curves are shown in the figure. Figure 19 .

[0160] Figure 19 In the above, MIL101 is MIL-101 (F / Cr=1) prepared in Comparative Example 1, MIL101 NH4F is MIL-101 NH4F (F / Cr=1) prepared in Comparative Example 2, PMA-MIL101 5% PMA is PMA-MIL-101 (5% PMA, F / Cr=1) prepared in Comparative Example 4, and PMA-MIL101 5% PMA NH4F is PMA-MIL-101 (5% PMA, F / Cr=1) NH4F prepared in Example 2.

[0161] Figure 19This further verifies that NH4F cleaning of PMA-MIL-101 can effectively remove excess PMA and free carboxylic acid from the pores. This is evidenced by comparing the weight loss of PMA-MIL-101 material at 100℃-400℃. Both MIL-101NH4F and PMA-MIL-101NH4F showed virtually no weight loss after NH4F cleaning in the 100℃-400℃ range; the weight loss in this temperature range is mostly due to the desorption and breaking of Cr-OH bonds. The framework of PMA-MIL-101NH4F only began to collapse at 400℃-500℃, demonstrating its good thermal stability. The final weight balance shows a significant reduction in weight loss after NH4F cleaning, indicating the formation of defects. Loading PMA further reduces the weight loss, indicating the formation of more ligand defects.

[0162] In the description of this application, it should be noted that the terms "upper", "lower", "inner", "outer", "front", "rear", "left", "right", etc., indicate the orientation or positional relationship based on the orientation or positional relationship in the working state of this application. They are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.

[0163] In the description of this application, it should be noted that, unless otherwise expressly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. Those skilled in the art can understand the specific meaning of these terms in this application based on the specific circumstances.

[0164] The present application has been described above with reference to preferred embodiments; however, these embodiments are merely exemplary and illustrative. Various substitutions and modifications can be made to the present application based on these embodiments, all of which fall within the protection scope of the present application.

Claims

1. A method for adsorption denitrification of oil products, characterized in that, The phosphomolybdic acid-MIL-101 composite material is dispersed in an oil product. The preparation method of the phosphomolybdic acid-MIL-101 composite material includes the following steps: (1) Provide a first mixture comprising a MIL-101 starting material mixture and phosphomolybdic acid, then perform hydrothermal synthesis and separate the intermediate solid product, wherein the MIL-101 starting material mixture comprises chromium nitrate, terephthalic acid, a monobasic acid and water, the chromium nitrate being Cr(NO3)3·9H2O, and the mass ratio of phosphomolybdic acid to the total mass of Cr(NO3)3·9H2O and terephthalic acid is (2-20):100; (2) The intermediate solid product obtained from step (1), NH4F and water are mixed, and then the solid product is separated, wherein the mass ratio of the intermediate solid product to NH4F is 1:(0.8-1.5) and the ratio of NH4F to water is 10mg:(0.5-1.5)ml.

2. The processing method according to claim 1, characterized in that, The monocarboxylic acid is selected from HF or HNO3.

3. The processing method according to claim 1, characterized in that, In the MIL-101 starting material mixture, the molar ratio of chromium nitrate, terephthalic acid, the monobasic acid, and water is 1:1:(0.4-1):(250-300).

4. The processing method according to claim 1, characterized in that, In step (1), the hydrothermal synthesis temperature is 210-220℃ and the time is 7-10h.

5. The processing method according to claim 1, characterized in that, In step (2), the mixing temperature is 55-65℃; In step (2), the mixing is a stirring mixture, the stirring speed is 350-650 rpm, and the time is 8-12 h.

6. The phosphomolybdic acid-MIL-101 composite material prepared by the method for preparing the phosphomolybdic acid-MIL-101 composite material in the oil adsorption denitrification treatment method according to any one of claims 1-5, characterized in that, The phosphomolybdic acid-MIL-101 composite material includes a MIL-101 substrate and phosphomolybdic acid composited in the MIL-101 substrate, wherein at least a portion of the phosphomolybdic acid is distributed inside the pores of the MIL-101 substrate.

7. The method for processing oil products according to claim 1, characterized in that, The mass ratio of the phosphomolybdic acid-MIL-101 composite material to the oil is (1-5):1000.

8. The method for processing oil products according to claim 1 or 7, characterized in that, The oil contains 200-500 ppm indole and / or 200-500 ppm quinoline.