Hydrogenolysis catalysts, methods of making and using the same, and methods of making cumene from alpha,alpha-dimethylbenzyl alcohol

By doping W onto a support to form amorphous low-polymerization WOx species and utilizing the synergistic effect of Pd and W, the conversion and selectivity of α,α-dimethylbenzyl alcohol hydrogenolysis to cumene are improved, solving the problems of insufficient stability and selectivity of existing catalysts and making it suitable for industrial applications.

CN117942978BActive Publication Date: 2026-11-24CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211330451.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-28
Publication Date
2026-11-24
Estimated Expiration
2042-10-28

AI Technical Summary

Technical Problem

Existing hydrogenolysis catalysts suffer from low conversion and low selectivity in the preparation of cumene from α,α-dimethylbenzyl alcohol. In particular, copper-based catalysts are prone to sintering at high temperatures, and non-precious metal catalysts are prone to generating byproducts, resulting in insufficient catalyst stability and selectivity.

Method used

A catalyst containing Pd and W is used. By directly doping W on the support, an amorphous low-polymerization WOx species is formed, which improves the dispersion of W. Furthermore, the catalytic activity and selectivity are enhanced through the synergistic effect of Pd and W.

Benefits of technology

It improves the conversion rate and product selectivity of hydrogenolysis reaction, making it suitable for industrial applications and solving the problems of catalyst stability and selectivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117942978B_ABST
    Figure CN117942978B_ABST
Patent Text Reader

Abstract

This invention relates to the field of catalysts, specifically to a hydrogenolysis catalyst, its preparation method and application, and a method for preparing cumene from α,α-dimethylbenzyl alcohol. The catalyst comprises: element Pd, element W, and a support; wherein the ultraviolet-Raman spectrum of the catalyst is at a wavenumber of 807 cm⁻¹. ‑1 wavenumber 714cm ‑1 wavenumber 273cm ‑1 The first signal peak exists at a wavenumber of 960-990 cm⁻¹. ‑1 A second signal peak exists at wavenumbers 300-360 cm⁻¹. ‑1 wavenumber 880-940cm ‑1 A third signal peak is present. In the catalyst preparation method of this invention, W doping is directly introduced into the preparation of the support, which is beneficial for the anchoring of the tungsten species WOx on the support and effectively improves the dispersibility of W. It is speculated that the tungsten species introduced by direct doping is amorphous, low-polymerization WO. X Species, the WO X Speciation is beneficial for improving catalyst activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of catalysts, specifically to a hydrogenolysis catalyst, its preparation method and application, and a method for preparing cumene from α,α-dimethylbenzyl alcohol. Background Technology

[0002] Propylene oxide (PO) is an important organic chemical raw material, mainly used in the production of polyether polyols, propylene glycol, and propylene glycol ethers. Currently, commercial PO production methods mainly include the chlorohydrin process, the co-oxidation process (PO / SM), the cumene peroxide recycling process (CHP), and the hydrogen peroxide direct oxidation process (HPPO). The CHP process for producing propylene oxide is unaffected by fluctuations in co-product prices, is environmentally friendly, requires minimal investment, and is a clean production process. It was first successfully developed by Sumitomo Chemical Co., Ltd. of Japan. The new PO production process using CHP as an oxidant includes steps such as cumene oxidation, propylene epoxidation, and α,α-dimethylbenzyl alcohol hydrogenolysis (DMBA).

[0003] In existing technologies, catalyst modification mainly focuses on improving the activity and selectivity of α,α-dimethylbenzyl alcohol hydrogenolysis, while less attention is paid to the stability of hydrogenolysis catalysts.

[0004] US664613B2 uses Cu-Cr oxide as a catalyst to produce cumene via hydrogenolysis of α,α-dimethylbenzyl alcohol with a conversion rate of up to 100% and a selectivity of up to 97.5%. However, copper-based catalysts are prone to sintering in reactions with high exothermic temperatures, and the long-term stability of the catalyst is problematic, which is not conducive to industrial applications.

[0005] CN114042460A uses niobium and tungsten to enhance the acidity of Ni-based catalysts, thereby improving the conversion rate and catalytic activity of non-precious metal catalytic systems. However, high Ni content can easily lead to the hydrogenation of benzene rings, generating isopropylcyclohexane, which reduces the selectivity of the catalyst.

[0006] As described above, this invention addresses the problem of low catalyst selectivity for cumene in existing cumene preparation technologies by providing a novel hydrogenolysis method for α,α-dimethylbenzyl alcohol, offering a possibility for achieving α,α-dimethylbenzyl alcohol hydrogenolysis in one step.

[0007] Existing technologies include W / Al2O3 catalytic systems prepared by the equal-volume impregnation method. It has been found that changes in calcination temperature lead to different aggregation states of the formed WOx, but this contributes little to the acidity of the catalyst and has limited effect on improving the catalyst activity. Summary of the Invention

[0008] The purpose of this invention is to overcome the problems of low reactant conversion and low product selectivity in existing hydrogenolysis catalysts, and to provide a hydrogenolysis catalyst, its preparation method and application, and a method for preparing cumene from α,α-dimethylbenzyl alcohol. This catalyst has the characteristics of high reactant conversion and high product selectivity.

[0009] To achieve the above objectives, a first aspect of the present invention provides a hydrogenolysis catalyst comprising: element Pd, element W, and a support; wherein the ultraviolet Raman spectrum of the catalyst is at wavenumber 807 cm⁻¹. -1 wavenumber 714cm -1 wavenumber 273cm -1 The first signal peak exists at wavenumbers 960-990 cm⁻¹. -1 A second signal peak exists at wavenumbers 300-360 cm⁻¹. -1 wavenumber 880-940cm -1 A third signal peak exists at this location.

[0010] A second aspect of the present invention provides a method for preparing the catalyst described herein, the method comprising:

[0011] a. Mix the carrier source, the precursor containing element W, the organic acid and the binder, then shape it, dry it first, and calcine it first to obtain the carrier;

[0012] b. Contact the support prepared in step a with a solution containing a precursor containing element Pd, filter, wash, then dry and calcine a second time to obtain the catalyst.

[0013] A third aspect of the present invention provides the use of the catalyst of the present invention in the hydrogenolysis of a feedstock having a structure as shown in formula (a).

[0014]

[0015] Wherein, R1 is selected from an aromatic group; R2 is selected from a C1-C4 alkyl group, preferably from a methyl or ethyl group; R3 is selected from a C1-C4 alkyl group, preferably from a methyl or ethyl group.

[0016] A fourth aspect of this invention provides a method for preparing cumene from α,α-dimethylbenzyl alcohol. Under the conditions described in this application, a raw material containing α,α-dimethylbenzyl alcohol and optionally a solvent is contacted with a hydrogen-containing gas stream for reaction. Preferably, the conditions for the contact reaction include:

[0017] The molar ratio of the hydrogen-containing gas stream (based on hydrogen) to the feedstock containing α,α-dimethylbenzyl alcohol (based on α,α-dimethylbenzyl alcohol) is not less than 4.5, preferably 5-10; and / or

[0018] The reaction temperature is 150-240℃, preferably 160-230℃; and / or

[0019] The reaction pressure is 0.5-5.0 MPa, preferably 1.0-4.0 MPa; and / or

[0020] The volume hourly space velocity (VHSV) of α,α-dimethylbenzyl alcohol is 1.0–10.0 h⁻¹. -1 Preferred 1-6h -1 ;

[0021] Preferably, the solvent is selected from cumene.

[0022] Through the above technical solution, the present invention has the following beneficial effects:

[0023] The catalyst with the features of this invention has the advantages of high reactant conversion rate and high product selectivity.

[0024] In the catalyst preparation method of this invention, W doping is directly introduced into the preparation of the support, which is beneficial to the anchoring of the tungsten species WOx on the support and effectively improves the dispersibility of W. It is speculated that the tungsten species introduced by direct doping is amorphous low-polymerization WO. X Species, the WO X Speciation is beneficial for improving catalyst activity.

[0025] When the catalyst of this invention was applied to the DMBA hydrogenolysis reaction, a synergistic effect between Pd and W was found, which can effectively improve the activity and selectivity of the DMBA hydrogenolysis reaction. Attached Figure Description

[0026] Figure 1 These are the ultraviolet Raman spectra of the catalysts prepared in Example 1 and Comparative Examples 2-3 of this invention;

[0027] Figure 2 These are the XRD patterns of the catalysts prepared in Example 1 and Comparative Examples 2-3 of this invention;

[0028] Figure 3 This is the NH3-TPD diagram of the catalysts in Example 1 and Comparative Example 1 of the present invention. Detailed Implementation

[0029] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0030] The first aspect of this invention provides a hydrogenolysis catalyst comprising: element Pd, element W, and a support; wherein the ultraviolet Raman spectrum of the catalyst is at a wavenumber of 807 cm⁻¹. -1 wavenumber 714cm -1 wavenumber 273cm -1 The first signal peak exists at wavenumbers 960-990 cm⁻¹. -1 A second signal peak exists at wavenumbers 300-360 cm⁻¹. -1 wavenumber 880-940cm -1 A third signal peak exists at this location.

[0031] Catalysts possessing the aforementioned characteristics of this invention have the advantages of high activity (high reactant conversion rate) and high product selectivity.

[0032] According to a preferred embodiment of the present invention, the intensity of the first signal peak in the ultraviolet Raman spectrum of the catalyst is 0-50.0% of the total intensity of the first and second signal peaks, and is not zero. By adopting the aforementioned preferred embodiment, the activity of the catalyst and the selectivity of the reactants can be further improved.

[0033] According to a preferred embodiment of the present invention, the XRD pattern of the catalyst does not have signal peaks at 2θ of 23.2°, 23.6°, and 24.2°.

[0034] According to a preferred embodiment of the present invention, the carrier is selected from at least one of alumina carrier, silica carrier and zirconium oxide carrier.

[0035] According to a preferred embodiment of the present invention, the catalyst comprises: 0.1-2.0 wt% of elemental Pd; 0.5-15 wt% of elemental W; and 84.9-97.5 wt% of support.

[0036] A second aspect of the present invention provides a method for preparing the catalyst described herein, the method comprising:

[0037] a. Mix the carrier source, the precursor containing element W, the organic acid and the binder, then shape it, dry it first, and calcine it first to obtain the carrier;

[0038] b. Contact the support prepared in step a with a solution containing a precursor containing element Pd, filter, wash, then dry and calcine a second time to obtain the catalyst.

[0039] In the catalyst preparation method of this invention, W doping is directly introduced into the preparation of the support, which is beneficial to the anchoring of the tungsten species WOx on the support and effectively improves the dispersibility of W. It is speculated that the tungsten species introduced by direct doping is amorphous low-polymerization WO. X Species, the WO XSpeciation is beneficial for improving catalyst activity.

[0040] In this invention, the forming method can be a conventional choice in the art. According to a preferred embodiment of the invention, the forming method includes kneading and extrusion.

[0041] In this invention, the range of precursors containing element W is relatively wide. According to a preferred embodiment of this invention, the precursor containing element W is a compound containing element W, preferably a tungstate, and more preferably selected from at least one of ammonium tungstate, ammonium paratungstate, and ammonium metatungstate.

[0042] In this invention, the range of Pd-containing precursors is relatively wide. According to a preferred embodiment of this invention, the Pd-containing precursor is a Pd-containing compound, preferably selected from at least one of palladium chloride, palladium nitrate, ammonium chloropalladate, ammonium chloropalladate, palladium acetate, and palladium sulfate.

[0043] According to a preferred embodiment of the present invention, the carrier source is selected from at least one of alumina carrier source, silicon oxide carrier source and zirconium oxide carrier source.

[0044] According to a preferred embodiment of the present invention, the organic acid is a C1-C6 organic acid, preferably selected from at least one of citric acid, acetic acid, and formic acid. By adopting the aforementioned preferred embodiment, the reactivity and product selectivity of the reaction can be further improved.

[0045] In this invention, the range of selectable binders is relatively wide. According to a preferred embodiment of this invention, the binder is selected from one or two of nitric acid and guar gum powder.

[0046] In this invention, the first drying conditions can be conventionally chosen in the art. According to a preferred embodiment of the invention, the first drying conditions include: a temperature of 60-120°C and a time of 2-24 hours, preferably a temperature of 80-100°C and a time of 4-12 hours. This embodiment of the invention uses a temperature of 90°C and a time of 8 hours as an example to illustrate the advantages of the invention.

[0047] In this invention, the conditions for the first roasting can be conventionally chosen in the art. According to a preferred embodiment of this invention, the conditions for the first roasting include: a temperature of 500-1200℃ and a time of 2-12 hours, preferably a temperature of 600-1000℃ and a time of 3-6 hours. This invention uses an example of a temperature of 800℃ and a time of 8 hours to illustrate the advantages of this invention.

[0048] In this invention, the second drying conditions can be conventionally chosen in the art. According to a preferred embodiment of the invention, the second drying conditions include: a temperature of 60-120°C and a time of 2-24 hours, preferably a temperature of 80-100°C and a time of 4-12 hours. This invention uses a temperature of 90°C and a time of 8 hours as an example to illustrate the advantages of the invention.

[0049] In this invention, the conditions for the second calcination can be conventionally chosen in the art. According to a preferred embodiment of this invention, the conditions for the second calcination include: a temperature of 300-800℃ and a time of 2-12 hours, preferably a temperature of 400-600℃ and a time of 4-12 hours. This invention uses a temperature of 500℃ and a time of 4 hours as an example to illustrate the advantages of this invention.

[0050] In this invention, the contact conditions can be conventionally chosen in the art. According to a preferred embodiment of the invention, the contact conditions include: a temperature of 30-100°C and a time of 10-60 minutes, preferably a temperature of 30-90°C and a time of 20-50 minutes. This invention uses an over-immersion method with a temperature of 50°C and a time of 20 minutes as an example to illustrate the advantages of the invention.

[0051] A third aspect of the present invention provides the use of the catalyst of the present invention in the hydrogenolysis of a feedstock having a structure as shown in formula (a).

[0052]

[0053] Wherein, R1 is selected from an aromatic group; R2 is selected from a C1-C4 alkyl group, preferably from a methyl or ethyl group; R3 is selected from a C1-C4 alkyl group, preferably from a methyl or ethyl group.

[0054] When the catalyst of this invention is applied to the hydrogenolysis reaction of the aforementioned raw materials, it exhibits excellent activity and product selectivity in the hydrogenolysis reaction.

[0055] A fourth aspect of the present invention provides a method for preparing cumene from α,α-dimethylbenzyl alcohol, wherein a raw material containing α,α-dimethylbenzyl alcohol and optionally a solvent is reacted with a hydrogen-containing gas stream in the presence of the catalyst described in the present invention.

[0056] In this invention, the conditions for the contact reaction can be conventionally chosen in the art.

[0057] According to a preferred embodiment of the present invention, the conditions for the contact reaction include: the molar ratio of the hydrogen-containing gas stream (calculated as hydrogen) to the raw material containing α,α-dimethylbenzyl alcohol (calculated as α,α-dimethylbenzyl alcohol) is not less than 4.5, preferably 5-10.

[0058] According to a preferred embodiment of the present invention, the conditions for the contact reaction include: a reaction temperature of 150-250°C, preferably 160-230°C.

[0059] According to a preferred embodiment of the present invention, the conditions for the contact reaction include: a reaction pressure of 0.1-5.0 MPa, preferably 1.0-4.0 MPa.

[0060] According to a preferred embodiment of the present invention, the conditions for the contact reaction include: a volume hourly space velocity (VHSV) of α,α-dimethylbenzyl alcohol of 1.0-10.0 h⁻¹. -1 Preferred 1-6h -1 .

[0061] By employing the aforementioned preferred contact conditions, the reaction activity and product selectivity can be further improved.

[0062] In this invention, the solvent can be a conventional choice in the art. In a preferred embodiment of this invention, the solvent is selected from cumene.

[0063] According to a preferred embodiment of the present invention, the content of α,α-dimethylbenzyl alcohol in the raw material containing α,α-dimethylbenzyl alcohol is 10-100 wt%, preferably 50-70 wt%.

[0064] According to a preferred embodiment of the present invention, the raw material containing α,α-dimethylbenzyl alcohol further contains 0.01-3.00 wt% α-methylstyrene.

[0065] In this invention, there are no particular restrictions on the source of the raw material containing α,α-dimethylbenzyl alcohol. According to a preferred embodiment of this invention, the raw material containing α,α-dimethylbenzyl alcohol is selected from at least one of the products of the cumene peroxide recycling process and the dicumene peroxide technology.

[0066] The present invention will be described in detail below through embodiments. Unless otherwise specified, the raw materials used in the following embodiments are all commercially available products.

[0067] The content of each component was analyzed by a 7890 gas chromatograph from Agilent Technologies, USA, and the quantitative determination was performed using the area normalization method.

[0068] Raman spectra were obtained using a Horiba JY LabRAMARAMIS laser Raman spectrometer with a laser wavelength of 532 nm and a grating of 1200 mm. -1 Spectral range 100-1200cm -1 .

[0069] The crystal structure and phase composition of the catalyst were determined by powder X-ray diffraction (XRD). The tests were performed on a Bruker D8 Advance X-ray diffractometer using a CuKα1 source (λ = 0.15405 nm) and a graphite monochromator, with a tube voltage of 40 kV, a tube current of 50 mA, and a scanning range of 5–90°.

[0070] Acidity curve: Ammonia adsorption-programmed temperature desorption (NH3-TPD) test was performed on a chemisorption analyzer (Altamira AMI-3300). 0.15 g of sample was weighed, purged with N2 at 600 °C for 60 min, cooled to 25 °C, and then purged with a 10% NH3 / N2 mixture for 30 min until NH3 adsorption was saturated. Physically adsorbed NH3 was then removed in a He atmosphere. Subsequently, the temperature was increased at 10 °C for 1 min. -1 The temperature was increased to 600℃, and a TCD detector was used to detect the change in the concentration of NH3 in the exhaust gas.

[0071] Method for calculating the conversion rate of α,α-dimethylbenzyl alcohol:

[0072] Conversion rate = (molar amount of α,α-dimethylbenzyl alcohol in the feed - molar amount of α,α-dimethylbenzyl alcohol in the product) / molar amount of α,α-dimethylbenzyl alcohol in the feed;

[0073] Methods for calculating the selectivity of cumene:

[0074] Selectivity = (molar amount of cumene in product - molar amount of cumene in feedstock) / (molar amount of α,α-dimethylbenzyl alcohol in feedstock - molar amount of α,α-dimethylbenzyl alcohol in product).

[0075] Example 1

[0076] Al₂O₃ raw powder was mixed with ammonium metatungstate aqueous solution, citric acid, and guar gum powder. The mixture was kneaded, extruded, dried at 90℃ for 8 hours, and calcined at 800℃ for 4 hours to obtain a W-containing alumina support (denoted as W-Al₂O₃). Using W-Al₂O₃ as the support and palladium chloride as the precursor, the support was added to a palladium chloride aqueous solution, stirred and heated to 50℃, impregnated for 20 minutes, filtered, washed with deionized water, dried at 90℃ for 8 hours, and calcined at 500℃ for 4 hours. Pd / W-Al₂O₃ was prepared by excess impregnation method, with a Pd content of 0.5 wt%, a W content of 7 wt%, and an alumina support content of 92.5 wt%. The UV-Raman spectrum of the catalyst was detected, as shown below. Figure 1 It can be seen that the ultraviolet Raman spectrum of the catalyst is at a wavenumber of 807 cm⁻¹. -1 wavenumber 714cm -1 wavenumber 273cm -1 The first signal peak exists at wavenumbers 960-990 cm⁻¹. -1A second signal peak exists at wavenumbers 300-360 cm⁻¹. -1 880-940cm -1 A third signal peak exists at this location, and the intensity of the first signal peak is 46% of the total intensity of the first and second signal peaks; XRD spectrum, as shown. Figure 2 No signal peaks are found at 2θ values ​​of 23.2°, 23.6°, and 24.2°; the acid curve is as follows. Figure 3 .

[0077] Example 2

[0078] The preparation method is the same as in Example 1, except that (using silica sol as the support source and acetic acid as the organic acid), the Pd / W-SiO2 prepared has a Pd content of 0.5 wt%, a W content of 10 wt%, and a silica support content of 89.5 wt%. The UV-Raman spectrum of the catalyst was detected, and the intensity of the first signal peak was 49% of the total intensity of the first and second signal peaks.

[0079] Example 3

[0080] The preparation method is the same as in Example 1, except that the Pd / W-Al2O3 prepared contains 0.5 wt% Pd, 4 wt% W, and 95.5 wt% alumina support. The UV-Raman spectrum of the catalyst was analyzed, and the intensity of the first signal peak was 34% of the total intensity of the first and second signal peaks.

[0081] Example 4

[0082] The preparation method is the same as in Example 1, except that the Pd / W-Al2O3 prepared contains 0.5 wt% Pd, 20 wt% W, and 79.5 wt% alumina support. The UV-Raman spectrum of the catalyst was analyzed, and the intensity of the first signal peak was 55.0% of the total intensity of the first and second signal peaks.

[0083] Example 5

[0084] Similar to Example 1, except that no organic acid was added during the preparation of the support, resulting in Pd / W-Al2O3 with a Pd content of 0.5 wt%, a W content of 7 wt%, and an alumina support content of 92.5 wt%. The UV-Raman spectrum of the catalyst was analyzed, and the intensity of the first signal peak was 51.3% of the total intensity of the first and second signal peaks.

[0085] Comparative Example 1

[0086] The preparation method is the same as in Example 1, except that ammonium metatungstate is not added when preparing the alumina support. The resulting Pd / Al2O3 catalyst contains 0.5 wt% Pd and 99.5 wt% alumina support. The UV-Raman spectrum of the catalyst showed no first, second, or third signal peaks. The acidity curve is shown below. Figure 3 .

[0087] Comparative Example 2

[0088] The preparation method is the same as in Example 1, except that ammonium metatungstate is not added when preparing the alumina support. The prepared alumina support is impregnated with an equal volume of ammonium metatungstate aqueous solution, dried at 90°C for 8 hours, and calcined at 800°C for 4 hours to obtain a W-modified alumina support (denoted as W / Al2O3). Using W / Al2O3 as the support, Pd is loaded to prepare W / Pd / Al2O3 using the same method, wherein the Pd content is 0.5 wt%, the W content is 7 wt%, and the alumina support content is 92.5 wt%. The UV-Raman spectrum of the catalyst is detected, as shown below. Figure 1 No first signal peak or third signal peak was observed. The XRD spectrum is as follows: Figure 2 Compared with Example 1, signal peaks exist at 2θ of 23.2°, 23.6°, and 24.2°.

[0089] Comparative Example 3

[0090] Similar to Comparative Example 2, but with the difference that Pd was loaded onto the prepared alumina support phase, and then W was loaded onto it to obtain a Pd / W / Al2O3-based catalyst. The Pd content was 0.5 wt%, the W content was 7 wt%, and the alumina support content was 92.5 wt%. The UV-Raman spectrum of the catalyst was detected, as shown below. Figure 1 The intensity of the first signal peak is 61.3% of the total intensity of the first and second signal peaks. No third signal peak was observed. (XRD spectrum, as shown) Figure 2 Compared with Example 1, signal peaks exist at 2θ of 23.2°, 23.6°, and 24.2°.

[0091] Example 6

[0092] The catalysts prepared in Examples 1-5 and Comparative Examples 1-3 were used for the hydrogenolysis of α,α-dimethylbenzyl alcohol to prepare cumene:

[0093] Catalyst evaluation method: The prepared catalyst was loaded into a fixed-bed reactor for hydrogenolysis. The catalyst was reduced at 160℃ for 8 h. The benzyl alcohol feedstock contained 51.00 wt% cumene, 46.00 wt% α,α-dimethylbenzyl alcohol, 0.075 wt% α-methylstyrene, and impurities. The reaction pressure was 2.0 MPa, the inlet temperature was 160℃, the H2 / benzyl alcohol molar ratio was 6.0, and the liquid hourly space velocity was 2 h⁻¹.-1 The liquid phase products were analyzed using an Agilent Technologies 7890 gas chromatograph. Quantification was performed using the area normalization method, and the conversion rate and selectivity were calculated.

[0094] Catalyst performance:

[0095]

[0096] Through Table 1 and Figure 3 The results show that the catalyst prepared by the method of the present invention has stronger acidity and exhibits higher catalytic activity and selectivity for the hydrogenolysis of α,α-dimethylbenzyl alcohol, making it suitable for industrial applications.

[0097] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A method for preparing cumene from α,α-dimethylbenzyl alcohol, characterized in that, In the presence of a catalyst, a feedstock containing α,α-dimethylbenzyl alcohol and optionally a solvent is reacted with a hydrogen-containing gas stream. The catalyst comprises: element Pd, element W, and a support; wherein, the ultraviolet Raman spectrum of the catalyst is at a wavenumber of 807 cm⁻¹. -1 wavenumber 714cm -1 wavenumber 273cm -1 The first signal peak exists at wavenumbers 960-990 cm⁻¹. -1 A second signal peak exists at wavenumbers 300-360 cm⁻¹. -1 wavenumber 880-940cm -1 A third signal peak exists at this location; The intensity of the first signal peak in the ultraviolet Raman spectrum of the catalyst is 0-50.0% of the total intensity of the first and second signal peaks, and is not 0; The XRD pattern of the catalyst showed no signal peaks at 2θ values ​​of 23.2°, 23.6°, and 24.2°. The catalyst comprises: 0.1-2.0 wt% of elemental Pd; 4-15 wt% of elemental W; and 84.9-97.5 wt% of support.

2. The method according to claim 1, wherein, The carrier is selected from at least one of alumina carrier, silica carrier, and zirconium oxide carrier.

3. The method according to claim 1, wherein, Methods for preparing catalysts include: a. Mix the carrier source, the precursor containing element W and the binder, then shape it, dry it first, and calcine it first to obtain the carrier; b. Contact the support prepared in step a with a solution containing a precursor containing element Pd, filter, wash, then dry and calcine a second time to obtain the catalyst.

4. The method according to claim 3, wherein, In step a, an organic acid is added during the mixing process.

5. The method according to claim 3 or 4, wherein, The precursor containing element W is a compound containing element W; and / or The precursor containing element Pd is a compound containing element Pd; and / or The carrier source is selected from at least one of alumina carrier source, silica carrier source, and zirconium oxide carrier source; and / or The organic acid is a C1-C6 organic acid; and / or The binder is selected from one or two of nitric acid and guar gum.

6. The method according to claim 5, wherein, The precursor containing element W is a tungstate; and / or The Pd-containing compound is selected from at least one of palladium chloride, palladium nitrate, ammonium chloropalladate, ammonium chloropalladate, palladium acetate, and palladium sulfate; and / or The organic acid is selected from at least one of citric acid, acetic acid, and formic acid.

7. The method according to claim 5, wherein, The precursor containing element W is selected from at least one of ammonium tungstate, ammonium paratungstate, and ammonium metatungstate.

8. The method according to claim 3 or 4, wherein, The first drying conditions include: a temperature of 60-120°C and a time of 2-24 hours; and / or The conditions for the first calcination include: a temperature of 500-1200℃ and a time of 2-12 hours; and / or The second drying conditions include: a temperature of 60-120°C and a time of 2-24 hours; and / or The conditions for the second calcination include: a temperature of 300-800℃ and a time of 2-12 hours; and / or The contact conditions include a temperature of 30-100℃ and a time of 10-60 minutes.

9. The method according to claim 3 or 4, wherein, The first drying conditions include: a temperature of 80-100℃ and a time of 4-12 hours; and / or The conditions for the first calcination include: a temperature of 600-1000℃ and a time of 3-6 hours; and / or The second drying conditions include: a temperature of 80-100°C and a time of 4-12 seconds; and / or The conditions for the second calcination include: a temperature of 400-600℃ and a time of 4-12 hours; and / or The contact conditions include a temperature of 30-90℃ and a time of 20-50 minutes.

10. The method according to any one of claims 1-4, wherein, The conditions for the contact reaction include: The molar ratio of the hydrogen-containing gas stream (based on hydrogen) to the feedstock containing α,α-dimethylbenzyl alcohol (based on α,α-dimethylbenzyl alcohol) is not less than 4.5; and / or The reaction temperature is 150-250℃; and / or The reaction pressure is 0.1-5.0 MPa; and / or The volume hourly space velocity (VHSV) of α,α-dimethylbenzyl alcohol is 1.0–10.0 h⁻¹. -1 ; and / or The solvent is selected from cumene.

11. The method according to claim 10, wherein, The molar ratio of the hydrogen-containing gas stream (calculated as hydrogen) to the feedstock containing α,α-dimethylbenzyl alcohol (calculated as α,α-dimethylbenzyl alcohol) is 5-10; and / or The reaction temperature is 160-230℃; and / or The reaction pressure is 1.0-4.0 MPa; and / or The volume hourly space velocity (VHSV) of α,α-dimethylbenzyl alcohol is 1–6 h⁻¹. -1 .

12. The method according to any one of claims 1-4, wherein, The α,α-dimethylbenzyl alcohol content in the raw material containing α,α-dimethylbenzyl alcohol is 10-100 wt%.

13. The method according to claim 12, wherein, The raw material containing α,α-dimethylbenzyl alcohol has an α,α-dimethylbenzyl alcohol content of 10-70 wt%.

14. The method according to claim 12, wherein, The raw material containing α,α-dimethylbenzyl alcohol also contains 0.01-1.00 wt% α-methylstyrene.

15. The method according to claim 12, wherein, The raw material containing α,α-dimethylbenzyl alcohol is selected from one or both of the products of the cumene peroxide recycling process and the dicumene peroxide technology.

Citation Information

Patent Citations

  • Scissors.

    US664613A

  • Doped Pd / Au shell catalyst, method for producing the same and use thereof

    CN102015103A