Hydrodehydrogenating bi-directional catalytic composition, process for the preparation and use thereof, and hydrodeoxygenation and dehydrogenation processes
By preparing a catalytic composition containing Al, Mo, and Ni, the problems of insufficient catalytic activity and high cost in the prior art have been solved, achieving efficient hydrogenation and dehydrogenation reactions and improving product selectivity.
Patent Information
- Application Number
- CN202211319078.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-26
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-10-26
AI Technical Summary
Existing technologies lack efficient and low-cost non-precious metal bidirectional catalysts for hydrogenation and dehydrogenation in organic liquid hydrogen storage, as they exhibit insufficient catalytic activity and poor product selectivity.
A catalytic composition containing Al, Mo, and Ni is used, and through a specific ratio and preparation method, Mo and Ni are uniformly dispersed on the Al surface to form a bidirectional catalytic composition for hydrogenation and dehydrogenation of nitrogen-containing heterocyclic organic compounds.
It achieves highly efficient hydrogenation and dehydrogenation catalytic activity, reduces catalyst cost, and improves product selectivity, approaching the catalytic performance of precious metals.
Smart Images

Figure CN117943034B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of organic liquid hydrogen storage, specifically to a bidirectional catalytic composition for hydrogenation and dehydrogenation, its preparation method and application, and methods for hydrogenation and dehydrogenation. Background Technology
[0002] Hydrogen, as a renewable energy source, is highly energy efficient and produces almost no waste. Therefore, it holds promise as an important way to improve energy efficiency, reduce dependence on fossil fuels, improve the ecological environment, and ensure energy security. Currently, there is an urgent need to develop sustainable and efficient large-scale hydrogen production technologies.
[0003] Hydrogen typically exists in a gaseous state and is flammable, explosive, and easily diffused, so safety during storage and transportation must be a top priority. Currently, the main storage and transportation methods are gaseous, liquid, and chemical. Gaseous hydrogen storage tanks are widely used in vehicles, cryogenic liquid hydrogen is widely used in the aerospace field, and chemical hydrogen storage technology is still in the research and development stage. There are small-scale demonstrations of organic liquid hydrogen storage and transportation abroad.
[0004] Gaseous and liquid hydrogen storage and transportation are based on physical methods. Gaseous hydrogen storage requires high airtightness and pressure resistance of tank materials, suffers from low hydrogen transportation efficiency, and is costly for long-distance transport. Liquid hydrogen storage requires high insulation properties of materials, resulting in high equipment costs. Chemical hydrogen storage utilizes the ability of the storage medium to react with hydrogen under certain conditions to form stable compounds, and then releases hydrogen by changing the conditions. This technology mainly includes organic liquid hydrogen storage, liquid ammonia hydrogen storage, coordination hydride hydrogen storage, inorganic hydrogen storage, and methanol hydrogen storage. Organic liquid hydrogen storage technology is considered a promising chemical hydrogen storage technology due to its readily available raw materials, good compatibility of hydrogen absorption and release product transportation equipment with traditional oil and gas transportation systems, low transportation costs, and lack of large-scale investment. It is also considered to avoid wasting existing oil and gas resources in future energy transitions. The main hydrogen carriers for organic liquid storage and transportation are aromatic compounds, among which heterocyclic aromatic compounds are widely studied because the hydrogen and organic products are easily separated.
[0005] CN111569901A discloses a method for preparing and applying a bimetallic catalyst for hydrogenation and dehydrogenation of organic hydrogen storage materials. The method involves mixing a metal oxide, graphene, and molecular sieve support with a solution of a non-noble metal precursor (Ni, Cu, Mg, Fe) or a noble metal precursor (Pt, Pd, Rh, Ru, Au) using an impregnation method. The mixture is then stirred, dried, calcined, and reduced to obtain the catalyst for hydrogen storage and dehydrogenation on an organic support. This catalyst exhibits advantages such as high activity, good stability, and low cost.
[0006] CN110841630A provides a hydrogenation and dehydrogenation catalyst for organic hydrogen storage materials, comprising an active component and a support. The active component is selected from one or more of platinum, lead, rhodium, ruthenium, gold, and palladium, and the support is selected from one or more of metal oxides, molecular sieves, and porous materials. In the hydrogenation reaction of organic hydrogen storage materials, the catalyst of this invention achieves a conversion rate of up to 98% for ethylcarbazole and a selectivity of up to 98% for dodecylhydroethylcarbazole. In the dehydrogenation reaction of organic hydrogen storage materials, the catalyst of this invention achieves a conversion rate of up to 91% for dodecylhydroethylcarbazole and a selectivity of up to 89% for ethylcarbazole.
[0007] To date, there are few reports on two-way catalysts involving the simultaneous dehydrogenation and hydrogenation of organic liquids, and they are mainly noble metal catalysts. There are no publicly reported two-way catalysts without noble metals. Summary of the Invention
[0008] The purpose of this invention is to overcome the existing problems of the lack of non-precious metal bidirectional catalysts in organic liquid hydrogen storage, high catalyst cost, insufficient catalytic activity, and poor product selectivity. This invention provides a bidirectional catalytic composition for hydrogenation and dehydrogenation, its preparation method and application, and hydrogenation and dehydrogenation methods. This bidirectional catalytic composition for hydrogenation and dehydrogenation can efficiently catalyze the hydrogenation and dehydrogenation of nitrogen-containing heterocyclic organic compounds with good product selectivity.
[0009] To achieve the above objectives, the first aspect of the present invention provides a bidirectional catalytic composition for hydroaddition and dehydrogenation, the composition comprising a first metal element and a second metal element, wherein the first metal element comprises Al, and the second metal element comprises Mo and Ni; the molar ratio of the second metal element to the first metal element is not higher than 1, and the molar ratio of Mo to Ni is 0.2-5:1;
[0010] The first metal element exists in an oxidized state, and the second metal element is at least partially dispersed in a metallic state on the surface of the first metal element; the average particle size of the second metal element is 1-100 nm.
[0011] A second aspect of the present invention provides a method for preparing a bidirectional catalytic composition for hydroaddition and dehydrogenation, comprising the following steps:
[0012] (1) The compound containing the second metal element is mixed with a solvent to obtain a first mixture;
[0013] The second metallic element includes Mo and Ni, and in compounds containing the second metallic element, the molar ratio of Mo to Ni is 0.2-5:1 (based on elemental composition).
[0014] (2) The first mixture and the alkaline solution are mixed a second time to obtain a second mixture;
[0015] (3) The second mixture, alcohol and oxide containing the first metal element are mixed in a third mixture and then heated to obtain a composition precursor powder;
[0016] The first metal element includes Al, and the amount of oxide containing the first metal element and the second mixture is such that, in terms of elements, the molar ratio of the second metal element to the first metal element is not higher than 1.
[0017] (4) The precursor powder of the composition is contacted with a hydrogen-containing atmosphere to obtain the hydrodehydrogenation bidirectional catalytic composition.
[0018] A third aspect of the present invention provides a bidirectional catalytic composition for hydroaddition and dehydrogenation prepared by the above-described preparation method.
[0019] The fourth aspect of the present invention provides the application of the bidirectional catalytic composition for hydrodehydrogenation described in the first or third aspect in organic liquid hydrogen storage.
[0020] The fifth aspect of the present invention provides a hydrogenation method, comprising: contacting a nitrogen-containing heterocyclic organic compound with hydrogen gas in the presence of a hydrogenation catalyst under hydrogenation reaction conditions;
[0021] The hydrogenation catalyst is the bidirectional catalytic composition for hydrogenation and dehydrogenation described in the first or third aspect.
[0022] The sixth aspect of the present invention provides a dehydrogenation method, comprising: contacting the hydrogenation product of a nitrogen-containing heterocyclic organic compound with a dehydrogenation catalyst under dehydrogenation reaction conditions to carry out a dehydrogenation reaction to obtain hydrogen gas;
[0023] The dehydrogenation catalyst is the bidirectional catalytic composition for hydrodehydrogenation described in the first or third aspect.
[0024] The beneficial effects obtained by the present invention through the above technical solution are as follows:
[0025] (1) The bidirectional catalytic composition for hydrogenation and dehydrogenation provided by the present invention has bidirectional catalytic function for hydrogenation / dehydrogenation. Under the synergistic effect of the first metal element and the second metal element, it has both high hydrogenation activity and high dehydrogenation activity. Moreover, its hydrogenation and dehydrogenation activities are close to those of noble metals and far higher than those of conventional non-noble metal catalysts.
[0026] (2) The preparation method of the hydrogenation / dehydrogenation bidirectional catalytic composition provided by the present invention makes the first metal component and the second metal component have the same micro-region element distribution, and the resulting composition has excellent hydrogenation / dehydrogenation performance.
[0027] (3) The hydrogenation and dehydrogenation method provided by the present invention can achieve efficient dehydrogenation and hydrogenation of organic liquids through a bidirectional catalytic composition that does not contain precious metals, which greatly reduces the raw material cost of organic liquid hydrogen storage and is conducive to further improving the efficiency of organic liquid hydrogen storage. Attached Figure Description
[0028] Figure 1 This is a TEM image of the catalytic composition A1 in Example 1;
[0029] Figure 2 Comparison of X-ray diffraction patterns of catalytic compositions A1, A2, and A3;
[0030] Figure 3 This is a TEM image of the catalytic composition A2 in Example 2;
[0031] Figure 4 It is the hydrogenation product of N-ethylcarbazole and the dehydrogenation product of the hydrogenation product. 1 H NMR spectrum. Detailed Implementation
[0032] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0033] In this invention, the term "room temperature" refers to 25±5℃.
[0034] The first aspect of the present invention provides a two-way catalytic composition for hydroaddition and dehydrogenation, the composition comprising a first metal element and a second metal element, wherein the first metal element comprises Al, and the second metal element comprises Mo and Ni; the molar ratio of the second metal element to the first metal element is not higher than 1, and the molar ratio of Mo to Ni is 0.2-5:1;
[0035] The first metal element exists in an oxidized state, and the second metal element is at least partially dispersed in a metallic state on the surface of the first metal element; the average particle size of the second metal element is 1-100 nm.
[0036] In this invention, the first metal element exists in an oxidized state, and the second metal element is at least partially dispersed in a metallic state uniformly on the surface of the first metal element. Preferably, Ni, Mo, and Al have the same micro-region elemental distribution, i.e., Ni, Mo, and Al are in close contact. The inventors discovered that through the synergistic effect of the first and second metal elements, excellent bidirectional catalytic function for hydrogenation / dehydrogenation can be obtained, far exceeding that of conventional non-noble metal catalysts.
[0037] It should be noted that in the hydroaddition and dehydrogenation bidirectional catalytic composition of the present invention, the second metal element exists at least partially in a metallic state. The present invention does not have a particular limitation on the amount of elemental Mo or elemental Ni present. As long as there is a portion of elemental Mo or elemental Ni, the composition can better catalyze the hydrogenation and dehydrogenation reactions and improve the selectivity of the full hydrogenation or full dehydrogenation products.
[0038] In this invention, Al existing in an oxidized state means that Al exists in the form of Al2O3. This invention does not have a special limitation on the crystal form of Al2O3 in the combination. For example, it can be selected from at least one of α-alumina, δ-alumina, γ-alumina, η-alumina, and θ-alumina, preferably α-alumina and / or γ-alumina.
[0039] The first metal element of this invention includes Mo and Ni. As long as Mo and Ni are included, this invention does not exclude the second metal element from containing elements other than Mo and Ni among non-precious metal elements.
[0040] According to a preferred embodiment of the present invention, the composition comprises Al, Ni, Mo, and O. In the above-mentioned preferred embodiment, it is advantageous to further improve the hydrodehydrogenation performance of the composition.
[0041] According to the present invention, in order to further enhance the synergistic effect of the first metal element and the second metal element, preferably, the molar ratio of the second metal element to the first metal element is not higher than 0.3, and more preferably 0.1-0.3:1. The inventors of the present invention have discovered that the first metal element and the second metal element can produce a better synergistic effect when in a specific ratio, which is more conducive to further improving the hydrogenation and dehydrogenation performance of the catalytic composition and improving the hydrogen storage efficiency.
[0042] In this invention, the presence of both Mo and Ni in the second metal element can enhance the catalytic activity of the composition for the hydrogenation and dehydrogenation of organic liquids, especially nitrogen-containing heterocyclic organic compounds. Preferably, the molar ratio of Mo to Ni is 0.5-2:1, and can be, for example, typical but not limiting ratios such as 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, and 2:1. In the above preferred embodiments, it is beneficial to improve the catalytic activity of the composition.
[0043] In this invention, the content of each component in the composition is determined by ICP.
[0044] In this invention, preferably, the average particle size of the second metal element is 20-100 nm.
[0045] In this invention, the average particle size of the second metal element is obtained by transmission electron microscopy. The specific testing method includes: taking 10 photos at 50k magnification, counting the longest diameter of all the grains of the second metal element within the field of view, and calculating its average value.
[0046] In this invention, preferably, the composition is in the form of granules and / or rods, more preferably granules. The inventors have found in their research that the control of the composition morphology can optimize the catalytic performance of the composition. Preferably, the composition has a dispersed granular morphology.
[0047] According to the present invention, the particle size of the composition can be selected within a wide range, and can be chosen according to actual production needs. Preferably, the particle size of the composition is 0.5-10 μm, more preferably 1-5 μm, and even more preferably 1-4 μm. In the present invention, "particle size of the composition" refers to the longest diameter passing through the interior of the particles of the composition. It can be understood that when the composition is rod-shaped, the particle size of the composition is the length of the rod.
[0048] In this invention, the morphology and particle size of the composition are characterized by TEM. Specific testing methods include: taking 10 photographs at 50k magnification, counting the longest diameter of the catalyst particles within the field of view, and calculating their average value.
[0049] According to the present invention, preferably, the specific surface area of the composition is 0.5-5 cm². 2 / g, preferably 1-5cm 2 / g.
[0050] In this invention, the specific surface area is measured by the BET method of nitrogen physical adsorption determination.
[0051] A second aspect of the present invention provides a method for preparing a bidirectional catalytic composition for hydroaddition and dehydrogenation, comprising the following steps:
[0052] (1) The compound containing the second metal element is mixed with a solvent to obtain a first mixture;
[0053] The second metallic element includes Mo and Ni, and in compounds containing the second metallic element, the molar ratio of Mo to Ni is 0.2-5:1 (based on elemental composition).
[0054] (2) The first mixture and the alkaline solution are mixed a second time to obtain a second mixture;
[0055] (3) The second mixture, alcohol and oxide containing the first metal element are mixed in a third mixture and then heated to obtain a composition precursor powder.
[0056] The first metal element includes Al, and the amount of oxide containing the first metal element and the second mixture is such that, in terms of elements, the molar ratio of the second metal element to the first metal element is not higher than 1.
[0057] (4) The precursor powder of the composition is contacted with a hydrogen-containing atmosphere to obtain the hydrodehydrogenation bidirectional catalytic composition.
[0058] The above preparation method can control the distribution of the first metal element and the second metal element, so that the first metal component and the second metal component have the same micro-region element distribution, thereby making the prepared composition have excellent hydrogenation / dehydrogenation performance.
[0059] According to the preparation method provided by the present invention, the selection of the first metal element and the second metal element is as described above, and will not be repeated here.
[0060] In this invention, preferably, in the compound containing the second metal element, the molar ratio of Mo to Ni is 0.5-2:1 (based on elemental composition).
[0061] In this invention, there is no special limitation on the amount of solvent used, as long as it can achieve the dispersion of each component. Preferably, the total mass concentration of the second metal element in the first mixture is 0.005-5 g / mL, and more preferably 0.01-1 g / mL.
[0062] In this invention, preferably, the compound containing the second metal element includes a nickel source and a molybdenum source; in this invention, there are no special requirements for the order of the first mixing, the nickel source and the molybdenum source can be mixed with the solvent separately, and then mixed to obtain the first mixture; or the nickel source and the molybdenum source can be mixed together with the solvent to obtain the first mixture, as long as the above-mentioned content requirements are met.
[0063] The selection range for the specific types of nickel and molybdenum sources is relatively wide, and they can be selected from any conventional substances well known to those skilled in the art. Preferably, the nickel source is selected from at least one of nickel chloride, nickel nitrate, nickel sulfate, nickel phosphate, nickel fluoroborate, nickel acetate, nickel acetylacetone, nickel aminosulfonate, and nickel citrate.
[0064] Preferably, the molybdenum source is selected from at least one of molybdic acid, phosphomolybdic acid, ammonium molybdate, and molybdenum chloride.
[0065] In this invention, the specific compounds selected for the nickel source and molybdenum source may also contain water of crystallization, which is well known to those skilled in the art and will not be described in detail here.
[0066] In this invention, the solvent can be selected from a wide range of options; preferably, the solvent is water.
[0067] To facilitate mixing, a co-solvent is preferably added to the first mixture; the co-solvent can be a conventional choice in the art and will not be described in detail here.
[0068] In this invention, the first mixing can be carried out using conventional methods in the art, such as mixing under stirring conditions, as long as the components are mixed uniformly. Preferably, the temperature of the first mixing is 10-60°C, more preferably 15-50°C.
[0069] In this invention, the alkaline solution can be an alkaline compound or an aqueous solution containing an alkaline compound; preferably, the alkaline solution is an aqueous solution containing an alkaline compound.
[0070] According to the present invention, the range of alkaline compounds is relatively wide. Preferably, the alkaline compound is an organic base and / or an inorganic base, and more preferably selected from at least one of sodium hydroxide, potassium hydroxide, calcium hydroxide, ammonia, ethylenediamine and isopropylamine; more preferably, ammonia.
[0071] According to the present invention, preferably, the concentration of the alkaline compound in the alkaline solution is 0.2-5 mol / L, more preferably 0.5-2 mol / L.
[0072] According to the present invention, preferably, the mass ratio of the first mixture to the alkali solution is 1-10:1, more preferably 2-5:1; within the above-mentioned preferred mass ratio range, it is beneficial to uniform particle growth.
[0073] According to the present invention, preferably, the temperature of the second mixing is 10-60°C, more preferably 20-50°C.
[0074] According to the present invention, preferably, the alcohol is a C2-C3 water-soluble alcohol; more preferably, a water-soluble diol; more preferably, at least one of ethylene glycol and propylene glycol; and most preferably, ethylene glycol. Using the above-mentioned preferred embodiments facilitates uniform particle growth, thereby resulting in a composition with excellent hydrogenation / dehydrogenation properties.
[0075] According to a preferred embodiment of the present invention, the alkaline compound is ammonia, and the alcohol is ethylene glycol. In this preferred embodiment, the synergistic effect of ammonia and ethylene glycol is beneficial to further improve the hydrogenation / dehydrogenation performance of the obtained composition. Preferably, the volume ratio of the second mixture to the alcohol is 0.1-1:1, more preferably 0.1-0.5:1.
[0076] In this invention, there are no special requirements for the order of the third mixing. The second mixture and the alcohol can be mixed first, and then the oxide containing the first metal element can be added. Alternatively, the alcohol and the oxide containing the first metal element can be added to the second mixture at the same time.
[0077] Preferably, the first mixing, the second mixing, and the third mixing are each carried out independently under stirring conditions. The present invention does not have special requirements for the stirring rate, as long as the components can be mixed evenly. For example, the stirring rate can be 100-1500 rpm each independently.
[0078] Preferably, the temperature of the third mixing is 20-80°C, more preferably 40-50°C.
[0079] In this invention, preferably, the oxide containing the first metal element is selected from at least one of α-alumina, δ-alumina, γ-alumina, η-alumina, and θ-alumina, and more preferably α-alumina and / or γ-alumina.
[0080] According to the present invention, preferably, the heating conditions include: a heating temperature of not less than 90°C, preferably 100-150°C, and a reaction time of 0.5-5h, preferably 0.5-4h.
[0081] Preferably, step (3) further includes: performing solid-liquid separation, washing, and drying on the product obtained by heating to obtain the precursor powder of the composition. In this invention, the solid-liquid separation, washing, and drying can be performed using conventional methods in the art, and this invention does not have any particular limitations on this.
[0082] Preferably, the washing solution is selected from water and / or ethanol. More preferably, the washing solution is water and ethanol, with a volume ratio of water to ethanol of 0.2-5:1.
[0083] Preferably, the drying temperature is 60-120℃, more preferably 80-100℃; the drying time is 6-48h, more preferably 12-24h.
[0084] According to the present invention, preferably, the hydrogen-containing atmosphere is hydrogen or a mixture of hydrogen and an inert gas; the inert gas is preferably selected from argon and / or nitrogen. For example, a mixture of hydrogen and argon.
[0085] Preferably, the hydrogen volume fraction in the hydrogen-containing atmosphere is 10-100%, and the gas volume is measured under standard conditions.
[0086] Preferably, in step (4), the conditions for contacting the precursor powder of the composition with a hydrogen-containing atmosphere include: a contact temperature of not less than 350°C, preferably 400-550°C, more preferably 450-500°C; a contact time of 0.5-5h, preferably 1-4h; and a hydrogen-containing atmosphere pressure of 0.01-2MPa, preferably 0.02-1MPa, more preferably 0.05-1MPa.
[0087] In this invention, in order to ensure uniform particle growth, preferably, the contact in step (4) includes: heating the catalyst precursor powder to the contact temperature at a heating rate of 2-5℃ / min under a hydrogen-containing atmosphere.
[0088] In this invention, in step (4), the contact between the composition precursor powder and the hydrogen-containing atmosphere can be carried out in a conventional apparatus in the art, such as a tube furnace.
[0089] Preferably, before the precursor powder of the composition comes into contact with the hydrogen-containing atmosphere, the air in the device is replaced with an inert gas; there is no special limitation on the amount of inert gas used, as long as it can replace the air in the device.
[0090] Preferably, the preparation method further includes: after the precursor powder of the composition is contacted with a hydrogen-containing atmosphere, the contact product is cooled to no higher than 50°C in the presence of an inert gas to obtain the hydrotreating / dehydrogenating dual-catalytic composition. Using the above preferred embodiments can avoid particle breakage and is beneficial to improving the hydrotreating / dehydrogenating performance of the composition.
[0091] A third aspect of the present invention provides a bidirectional catalytic composition for hydroaddition and dehydrogenation prepared by the above-described preparation method.
[0092] The fourth aspect of the present invention provides the application of the hydrodehydrogenation bidirectional catalytic composition described in the first or third aspect in organic liquid hydrogen storage.
[0093] The fifth aspect of the present invention provides a hydrogenation method, comprising: contacting a nitrogen-containing heterocyclic organic compound with hydrogen gas in the presence of a hydrogenation catalyst under hydrogenation reaction conditions;
[0094] The hydrogenation catalyst is the bidirectional catalytic composition for hydrogenation and dehydrogenation described in the first or third aspect.
[0095] In this invention, preferably, the hydrogenation reaction conditions include: a reaction temperature of 50-200°C, more preferably 130-200°C; and a weight hourly space velocity (WHSV) of 0.5-50 h⁻¹ for nitrogen-containing heterocyclic organic compounds. -1 Preferably 1-30h -1 The hydrogen pressure is 2-10 MPa, preferably 5-8 MPa.
[0096] In this invention, the selection range of the nitrogen-containing heterocyclic organic compounds is relatively wide, and they can be selected from any nitrogen-containing heterocyclic organic compounds capable of hydrogen storage. Preferably, the nitrogen-containing heterocyclic organic compounds are selected from at least one of indole, quinoline, isoquinoline, N-alkylcarbazole, and alkyl-substituted carbazoles on the benzene ring.
[0097] In this invention, the alkyl-substituted carbazole on the benzene ring refers to a carbazole compound having an alkyl substitution on the benzene ring. Preferably, the alkyl-substituted carbazole on the benzene ring is 2-methylcarbazole and / or 3-methylcarbazole.
[0098] Preferably, the N-alkylcarbazole is N-methylcarbazole and / or N-ethylcarbazole.
[0099] The sixth aspect of the present invention provides a dehydrogenation method, comprising: contacting the hydrogenation product of a nitrogen-containing heterocyclic organic compound with a dehydrogenation catalyst under dehydrogenation reaction conditions to carry out a dehydrogenation reaction to obtain hydrogen gas;
[0100] The dehydrogenation catalyst is the bidirectional hydrodehydrogenation catalytic composition described in the first or third aspect;
[0101] Preferably, the dehydrogenation reaction conditions include: a reaction temperature of 100-250℃, more preferably 150-200℃, and a weight hourly space velocity (WHSV) of 0.5-50 h⁻¹ for the hydrogenation products of nitrogen-containing heterocyclic organic compounds. -1 Preferably 1-30h -1 The reaction pressure is 0.1-2 MPa, preferably 0.1-1 MPa.
[0102] In this invention, the selection range of the nitrogen-containing heterocyclic organic compounds is the same as that in the above-mentioned hydrogenation reaction, and will not be repeated here.
[0103] According to the present invention, the hydrogenation product of the nitrogen-containing heterocyclic organic compound can be a partially hydrogenated product or a fully hydrogenated product. For example, the nitrogen-containing heterocyclic organic compound is N-ethylcarbazole. It is understood that, depending on the degree of hydrogenation, the hydrogenation product of N-ethylcarbazole can be one or more of tetrahydro-N-ethylcarbazole, octahydro-N-ethylcarbazole, and dodecahydro-N-ethylcarbazole, or a mixture thereof.
[0104] Preferably, the contact is carried out under hydrogen-exposed or non-hydrogen-exposed conditions. Preferably, under hydrogen-exposed conditions, the volume hourly space velocity (VHSV) of hydrogen is 0.5-10 h⁻¹. -1 Preferably 2-5h -1 .
[0105] This invention also provides a method for continuous hydrogenation / dehydrogenation of nitrogen-containing heterocyclic organic compounds, comprising:
[0106] S1. Under hydrogenation reaction conditions, in the presence of a first catalyst, nitrogen-containing heterocyclic organic compounds are contacted with hydrogen-containing gas to undergo hydrogenation, thereby obtaining hydrogenation products of nitrogen-containing heterocyclic organic compounds.
[0107] Preferably, the hydrogenation reaction conditions include: a reaction temperature of 50-200℃, more preferably 130-200℃; and a weight hourly space velocity (WHSV) of 0.5-50 h⁻¹ for nitrogen-containing heterocyclic organic compounds. -1 Preferably 1-30h -1 The hydrogen pressure is 2-10 MPa, preferably 5-8 MPa.
[0108] S2. Under dehydrogenation reaction conditions, the hydrogenation product of the nitrogen-containing heterocyclic organic compound is contacted with a second catalyst to carry out a dehydrogenation reaction to obtain hydrogen gas;
[0109] Preferably, the dehydrogenation reaction conditions include: a reaction temperature of 100-250℃, more preferably 150-200℃, and a weight hourly space velocity (WHSV) of 0.5-50 h⁻¹ for the hydrogenation products of nitrogen-containing heterocyclic organic compounds. -1 Preferably 1-30h -1 The reaction pressure is 0.1-2 MPa, preferably 0.1-1 MPa.
[0110] Wherein, the first catalyst and the second catalyst are each independently selected from the hydrodehydrogenation bidirectional catalytic composition described in the first aspect or the third aspect.
[0111] Preferably, the nitrogen-containing heterocyclic organic compound is selected from at least one of indole, quinoline, isoquinoline, N-alkylcarbazole, and alkyl-substituted carbazole on a benzene ring, more preferably at least one of 2-methylcarbazole, 3-methylcarbazole, N-methylcarbazole, and N-ethylcarbazole, and more preferably N-ethylcarbazole.
[0112] The present invention will be described in detail below through embodiments.
[0113] The raw materials used in the following examples and comparative examples were all commercially available and had a purity >99%; the purity of hydrogen and argon was ≥99.999%, and the purity of hydrogen and argon was obtained by mass spectrometry analysis.
[0114] In each example and comparative example, the content of each component in the composition was determined by ICP.
[0115] The composition of the hydrogenation product and the dehydrogenation product of N-ethylcarbazole are both composed of... 1 H NMR determination.
[0116] Example 1
[0117] (1) Weigh a certain amount of nickel nitrate hexahydrate and ammonium heptahydrate tetrahydrate according to the Mo / Ni stoichiometric ratio of 1:1 using an electronic balance. The total mass is 10 grams. Add 25 mL of deionized water to obtain the first mixture. The first mixing temperature is 50℃.
[0118] (2) Add 10 mL of 2 mol / L dilute ammonia water to the first mixture above, and carry out the second mixing at 50°C to form a clear solution, and then obtain the second mixture.
[0119] (3) Add 250 mL of ethylene glycol and 15 g of γ-alumina to the second mixture. After stirring evenly with a magnetic stirrer at 50 °C, the stirring speed is 300 rpm. Transfer to a round-bottom flask and keep stirring. React at a constant temperature of 120 °C in an oil bath for 30 min. After the liquid in the flask turns into a suspension, filter to obtain the precursor powder of the catalytic composition. Wash the separated precursor powder three times with deionized water and ethanol at a volume ratio of 1:1. Dry at 80 °C for 12 h to obtain the precursor powder of the composition.
[0120] (4) 1g of catalyst precursor was placed in a small porcelain boat into a quartz tube furnace. Ar was first passed through the furnace at room temperature for 30 min, and then Ar and H2 flow rates were increased to 50 mL / min. -1 and 30mL min -1 In a mixed atmosphere at 10℃ min -1 The temperature was increased to 450℃ at a rate of 1 MPa, and held at this temperature for 2 hours. Then, the H2 flow was stopped, and Ar flow was continued to reduce the temperature of the tube furnace to below 50℃, yielding the catalytic composition sample A1. The composition of A1 is shown in Table 1.
[0121] TEM image of A1 as follows Figure 1 As shown, the elements are evenly distributed. The XRD pattern of A1 is as follows. Figure 2 As shown, it exhibits a high degree of crystallinity. Due to the high dispersion of Ni and Mo, their XRD diffraction peak signals are submerged among other diffraction signals.
[0122] Example 2
[0123] The method described in Example 1 was followed, except that the amount of γ-alumina used was 5 g, and the catalytic composition sample A2 was prepared. The composition of A2 is shown in Table 1. The XRD pattern of A2 is shown in Table 1. Figure 2 As shown in the figure. TEM characterization reveals that the catalyst has a rod-like morphology, such as... Figure 3 As shown. The length of the rod is denoted as the particle size of the rod-shaped particle.
[0124] Example 3
[0125] The method was followed as in Example 1, except that the amount of γ-alumina used was 25 g, and the catalytic composition sample was A3. A3 had a particulate morphology, and the XRD pattern of A3 is shown below. Figure 2 As shown in Table 1.
[0126] Example 4
[0127] (1) Weigh a certain amount of nickel nitrate hexahydrate and ammonium heptahydrate tetrahydrate according to the Mo / Ni stoichiometric ratio of 1:2 using an electronic balance. The total mass is 10g. Add 25mL of deionized water to obtain the first mixture. The first mixing temperature is 50℃.
[0128] (2) Add 10 mL of 3 mol / L dilute ammonia water to the first mixture above, and carry out the second mixing at 50°C to form a clear solution, and then obtain the second mixture.
[0129] (3) Add 250 mL of ethylene glycol and 15 g of γ-alumina to the second mixture. After stirring evenly with a magnetic stirrer at 50 °C, the stirring speed is 300 rpm. Transfer to a round-bottom flask and keep stirring. React at a constant temperature of 120 °C in an oil bath for 30 min. After the liquid in the flask turns into a suspension, filter to obtain the precursor powder of the catalytic composition. Wash the obtained precursor powder three times with deionized water and ethanol at a volume ratio of 2:1. Dry at 80 °C for 12 h to obtain the precursor powder of the composition.
[0130] (4) 1g of catalyst precursor was placed in a small porcelain boat into a quartz tube furnace. Ar was first passed through the furnace at room temperature for 30 min, and then Ar and H2 flow rates were increased to 50 mL / min. -1 and 30mL min -1 In a mixed atmosphere at 10℃ min -1 The temperature was increased to 450℃ at a rate of 1 MPa, and held at this temperature for 2 hours. Then, the H2 flow was stopped, and Ar flow was continued until the tube furnace temperature dropped below 50℃. Catalytic composition sample A4 was obtained. The composition of A4 is shown in Table 1.
[0131] Example 5
[0132] The method of Example 1 was followed, except that an equal amount of ethanol was used to replace ethylene glycol, resulting in catalyst A5. The composition of A5 is shown in Table 1.
[0133] Example 6
[0134] (1) Weigh a certain amount of nickel nitrate hexahydrate and ammonium molybdate heptahydrate according to the Mo / Ni stoichiometric ratio of 2:1 using an electronic balance. The total mass is 10g. Add 25mL of deionized water to obtain the first mixture. The first mixing temperature is 50℃.
[0135] (2) Add 10 mL of 3 mol / L dilute ammonia water to the first mixture above, and carry out the second mixing at 50°C to form a clear solution, and then obtain the second mixture.
[0136] (3) Add 250 mL of ethylene glycol and 15 g of γ-alumina to the second mixture. After stirring evenly with a magnetic stirrer at 50 °C, transfer to a round-bottom flask and keep stirring. React at a constant temperature of 120 °C in an oil bath for 30 min. After the liquid in the flask turns into a suspension, filter to obtain the precursor powder of the catalytic composition. Wash the separated precursor powder three times with deionized water and ethanol at a volume ratio of 2:1 and dry at 80 °C for 12 h to obtain the precursor powder of the composition.
[0137] (4) 1g of catalyst precursor was placed in a small porcelain boat into a quartz tube furnace. Ar was first passed through the furnace at room temperature for 30 min, and then Ar and H2 flow rates were increased to 50 mL / min. -1 and 30mL min -1 In a mixed atmosphere at 10℃ min -1 The temperature was increased to 450℃ at a rate of 1 MPa, and held at this temperature for 2 hours. Then, the H2 flow was stopped, and Ar flow was continued until the tube furnace temperature dropped below 50℃. Catalytic composition sample A5 was obtained. The composition of A5 is shown in Table 1.
[0138] Comparative Example 1
[0139] The method of Example 1 was followed, except that no alcohol or base was added. The resulting composition was designated DA1, and its composition is shown in Table 1.
[0140] Comparative Example 2
[0141] (1) According to the Mo / Ni stoichiometric ratio of 1:1, a certain amount of nickel nitrate hexahydrate and ammonium heptamolybdate tetrahydrate totaling 10 g were weighed using an electronic balance, and 25 mL of deionized water was added to obtain the first mixture. The first mixing temperature was 50 °C.
[0142] (2) Add 250 mL of ethylene glycol to the first mixture above, and carry out a second mixing at 50 °C to form a clear solution, thereby obtaining the second mixture;
[0143] (3) Add 10 mL of 2 mol / L dilute ammonia and 15 g of γ-alumina to the second mixture. After stirring evenly with a magnetic stirrer at 50 °C, the stirring speed is 300 rpm. Transfer to a round-bottom flask and keep stirring. React at a constant temperature of 120 °C in an oil bath for 30 min. After the liquid in the flask turns into a suspension, filter to obtain the precursor powder of the catalytic composition. Wash the obtained precursor powder three times with deionized water and ethanol at a volume ratio of 1:1. Dry at 80 °C for 12 h to obtain the precursor powder of the composition.
[0144] (4) 1g of catalyst precursor was placed in a small porcelain boat into a quartz tube furnace. Ar was first passed through the furnace at room temperature for 30 min, and then Ar and H2 flow rates were increased to 50 mL / min. -1 and 30mL min -1 In a mixed atmosphere at 10℃ min -1 The temperature was increased to 450℃ at a rate of 1 MPa, and held at this temperature for 2 hours. Then, the H2 flow was stopped, and Ar flow was continued to reduce the temperature of the tube furnace to below 50℃, yielding the catalytic composition sample DA2. The composition of DA2 is shown in Table 1.
[0145] Table 1
[0146]
[0147]
[0148] Test case
[0149] The catalytic compositions of the embodiments and comparative examples of the present invention were used to conduct hydrogenation experiments of N-ethylcarbazole (NEC).
[0150] The hydrogenation reaction was carried out in a high-pressure reactor under the following conditions: reaction temperature 180℃, reaction pressure 7MPa, and weight hourly space velocity (WHSV) of N-ethylcarbazole (NEC) 0.5 h⁻¹. -1 The reaction time was 20 hours, and the pressure sensor count p was recorded as a time t curve. Based on the initial t curve data obtained from the test, the hydrogen absorption was calculated using Formula 1 and Formula 2, and finally, the curve showing the change of hydrogen absorption of the reaction substrate over time was obtained.
[0151] Formula 1: n=ΔpV / RT, where T is the reaction temperature, Δp is the pressure change during the reaction, and V is the volume of the reactor cavity.
[0152] Formula 2: C = 100 × n × 2 / M, where M is the mass of the substrate N-ethylcarbazole (NEC), and C is the amount of hydrogen absorbed by the catalyst. The product composition was determined by NMR after the reaction, and the Ct curve was corrected by combining the relative proportions of several products with the total amount of feedstock.
[0153] The content of NEC's hydrogen absorption products, tetrahydro-N-ethylcarbazole (4H-NEC), octahydro-N-ethylcarbazole (8H-NEC), and dodecahydro-N-ethylcarbazole (12H-NEC), can be determined by... 1 Peaks at specific positions in H NMR were identified, and the content of each product and the total hydrogen absorption of the NEC hydrogenation reaction were calculated based on the area ratio.
[0154] like Figure 4 As shown, the chemical shifts of the H atoms attached to the benzene ring in NEC, 4H-NEC, 8H-NEC, and 12H-NEC are at positions ranging from 1.07 to 0.90 ppm. The chemical shifts of the H atoms on the methylene group attached to the N atom are different: NEC has a quartet of about 4.4 ppm, 4H-NEC has about 4.1 ppm, and 8H-NEC has about 3.7 ppm, while 12H-NEC has about 2.6 ppm.
[0155] The contents of each substance and the total hydrogen absorption in the hydrogenation reaction products of nitrogen-containing heterocyclic compounds were calculated according to Formula 3-5, and the results are shown in Table 2:
[0156] Formula 3: Product mole percentage = S n / (S1+S2+S3+S4), where n is 1-4.
[0157] Formula 4: Total hydrogen absorption = (4S2 + 8S3 + 12S4)M1 / (S1 + S2 + S3 + S4), where M1 is the number of NEC moles.
[0158] Wherein S1 is the peak area at chemical shift 4.4 (NEC), S2 is the peak area at chemical shift 4.1 (4H-NEC), S3 is the peak area at chemical shift 3.7 (8H-NEC), and S4 (12H-NEC) is the peak area at chemical shift 2.6.
[0159] Table 2
[0160]
[0161] The above-mentioned catalyst was used to conduct dehydrogenation experiments on the hydrogenation products of N-ethylcarbazole (NEC).
[0162] The hydrogenation product of N-ethylcarbazole (NEC) is the 12H-NEC product from the above hydrogenation experiment.
[0163] The reaction temperature was 200℃, the pressure was atmospheric pressure, the reaction time was 40 min, and the weight hourly space velocity (WHSV) of the hydrogenation product of N-ethylcarbazole (NEC) was 0.5 h⁻¹. -1 Record the instantaneous hydrogen release flow rate q as a function of time t. After hydrogen release is complete, integrate the instantaneous flow rate q with respect to time t to obtain the Qt curve showing the total hydrogen release flow rate Q as a function of time t. Calculate the molar percentage of each substance in the product according to Formula 3. Correct the total hydrogen release amount according to Formula 5, and the results are shown in Table 3.
[0164] Formula 5: Total hydrogen release = (12S2 + 8S3 + 4S4)M4 / (S1 + S2 + S3 + S4), where M4 is the number of moles of 12H-NEC.
[0165] The results of the hydrogen charging and discharging examples and comparative examples are shown in Table 1. The total hydrogen absorption represents the degree of hydrogen absorption under specific reaction conditions, with a maximum value of 5.8 wt%, corresponding to the conversion of all N-ethylcarbazole to 12H-NEC. The total hydrogen release represents the degree of hydrogen release under specific conditions, with a maximum value of 5.5 wt%, corresponding to the conversion of all 12H-NEC to N-ethylcarbazole.
[0166] Hydrogen release / absorption efficiency (%) = (total hydrogen release / M4) / (total hydrogen absorption / M1)×100%.
[0167] Table 3
[0168] Example number Total hydrogen absorption (wt%) Total hydrogen release (wt%) Hydrogen absorption / desorption efficiency % Example 1 5.45 4.84 83.66 Example 2 2.63 2.26 80.96 Example 3 2.88 1.91 62.48 Example 4 2.73 2.61 90.07 Example 5 3.10 2.75 83.57 Example 6 2.65 2.42 86.03 Comparative Example 1 0.55 0.12 20.55 Comparative Example 2 1.49 0.46 29.08
[0169] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A bidirectional catalytic composition for hydroaddition and dehydrogenation, characterized in that, The composition includes a first metallic element and a second metallic element, wherein the first metallic element includes Al and the second metallic element includes Mo and Ni; In terms of elements, the molar ratio of the second metallic element to the first metallic element is not higher than 1, and the molar ratio of Mo to Ni is 0.2-5:1; The first metal element exists in an oxidized state, and the second metal element is at least partially dispersed in a metallic state on the surface of the first metal element; the average particle size of the second metal element is 20-100 nm. The composition is in the form of granules and / or rods; when the composition is in the form of rods, the particle size of the composition is the length of the rod; the particle size of the composition is 0.5-10 μm.
2. The composition according to claim 1, wherein, The molar ratio of the second metallic element to the first metallic element is no higher than 0.
3.
3. The composition according to claim 2, wherein, The molar ratio of the second metallic element to the first metallic element is 0.1-0.3:
1.
4. The composition according to claim 1 or 2, wherein, The molar ratio of Mo to Ni is 0.5-2:
1.
5. The composition according to claim 1 or 2, wherein, The composition is in granular form.
6. The composition according to claim 1 or 2, wherein, The particle size of the composition is 1-5 μm.
7. A method for preparing the hydrodehydrogenation bidirectional catalytic composition according to any one of claims 1-6, characterized in that, Includes the following steps: (1) The compound containing the second metal element and the solvent are mixed for the first time to obtain a first mixture; Wherein, the second metallic element includes Mo and Ni; in the compound containing the second metallic element, the molar ratio of Mo to Ni is 0.2-5:1, based on elemental composition; (2) The first mixture and the alkaline solution are mixed a second time to obtain a second mixture; (3) The second mixture, alcohol and oxide containing the first metal element are mixed in a third mixture and then heated to obtain a composition precursor powder; The first metal element includes Al, and the amount of oxide containing the first metal element and the second mixture is such that, in terms of elements, the molar ratio of the second metal element to the first metal element is not higher than 1. (4) The precursor powder of the composition is contacted with a hydrogen-containing atmosphere to obtain the hydrodehydrogenation bidirectional catalytic composition.
8. The preparation method according to claim 7, wherein, In compounds containing a second metallic element, the molar ratio of Mo to Ni, calculated by element, is 0.5-2:
1.
9. The preparation method according to claim 7, wherein, In the first mixture, the total mass concentration of the second metal element is 0.005-5 g / mL.
10. The preparation method according to claim 9, wherein, In the first mixture, the total mass concentration of the second metal element is 0.01-1 g / mL.
11. The preparation method according to claim 7, wherein, The compound containing the second metallic element includes nickel and molybdenum sources.
12. The preparation method according to claim 11, wherein, The nickel source is selected from at least one of nickel chloride, nickel nitrate, nickel sulfate, nickel phosphate, nickel fluoroborate, nickel acetate, nickel acetylacetone, nickel aminosulfonate, and nickel citrate.
13. The preparation method according to claim 11, wherein, The molybdenum source is selected from at least one of molybdic acid, phosphomolybdic acid, ammonium molybdate, and molybdenum chloride.
14. The preparation method according to claim 7, wherein, The solvent is water.
15. The preparation method according to claim 7, wherein, The temperature of the first mixture is 10-60℃.
16. The preparation method according to claim 15, wherein, The temperature of the first mixture is 15-50℃.
17. The preparation method according to any one of claims 7-16, wherein, The alkaline solution is an aqueous solution containing an alkaline compound.
18. The preparation method according to claim 17, wherein, The alkaline compound is an organic base and / or an inorganic base.
19. The preparation method according to claim 18, wherein, The alkaline compound is selected from at least one of sodium hydroxide, potassium hydroxide, calcium hydroxide, ammonia, ethylenediamine, and isopropylamine.
20. The preparation method according to claim 17, wherein, The alkaline solution contains alkaline compounds at a concentration of 0.2-5 mol / L. And / or, the volume ratio of the first mixture to the alkali solution is 1-10:
1. And / or, the temperature of the second mixture is 10-60°C.
21. The preparation method according to claim 20, wherein, The concentration of the alkaline compound in the alkaline solution is 0.5-2 mol / L; And / or, the volume ratio of the first mixture to the alkaline solution is 2-5:1; And / or, the temperature of the second mixture is 20-50°C.
22. The preparation method according to any one of claims 7-16, wherein, The amounts of the oxide containing the first metallic element and the second mixture are such that, elementally, the molar ratio of the second metallic element to the first metallic element is not higher than 0.
3. And / or, the alcohol is a C2-C3 water-soluble alcohol; And / or, the volume ratio of the second mixture to the alcohol is 0.1-1:1; And / or, the first mixture, the second mixture, and the third mixture are each carried out independently under stirring conditions, wherein the stirring rate is each independently 100-1500 rpm; And / or, the temperature of the third mixture is 20-80°C.
23. The preparation method according to claim 22, wherein, The amount of the oxide containing the first metal element and the second mixture is such that, in terms of elements, the molar ratio of the second metal element to the first metal element is 0.1-0.3:1; And / or, the alcohol is a water-soluble diol; And / or, the volume ratio of the second mixture to the alcohol is 0.1-0.5:1; And / or, the temperature of the third mixture is 40-50°C.
24. The preparation method according to claim 23, wherein, The alcohol is ethylene glycol and / or propylene glycol.
25. The preparation method according to any one of claims 7-16, wherein, The oxide containing the first metallic element is selected from at least one of α-alumina, δ-alumina, γ-alumina, η-alumina, and θ-alumina; And / or, the heating conditions include: a heating temperature not lower than 90°C; And / or, step (3) further includes: performing solid-liquid separation, washing and drying on the product obtained by heating to obtain the precursor powder of the composition.
26. The preparation method according to claim 25, wherein, The heating conditions include: a heating temperature of 100-150℃ and a reaction time of 0.5-4h.
27. The preparation method according to any one of claims 7-16, wherein, The hydrogen-containing atmosphere is hydrogen gas or a mixture of hydrogen gas and an inert gas.
28. The preparation method according to claim 27, wherein, The hydrogen volume fraction in the hydrogen-containing atmosphere is 10-100%, and the gas volume is measured under standard conditions.
29. The preparation method according to any one of claims 7-16, wherein in step (4), the conditions for contacting the precursor powder of the composition with a hydrogen-containing atmosphere include: The contact temperature should not be lower than 350℃; the contact time should be 0.5-5 hours. The pressure of the hydrogen-containing atmosphere is 0.01-2 MPa.
30. The preparation method according to claim 29, wherein, In step (4), the conditions for contacting the precursor powder of the composition with a hydrogen-containing atmosphere include: a contact temperature of 400-550°C; a contact time of 1-4 hours; and a hydrogen-containing atmosphere pressure of 0.02-1 MPa.
31. The preparation method according to claim 30, wherein, In step (4), the conditions for contacting the precursor powder of the composition with a hydrogen-containing atmosphere include: a contact temperature of 450-500°C and a hydrogen-containing atmosphere pressure of 0.05-1 MPa.
32. The hydrodehydrogenation bidirectional catalytic composition prepared by the method according to any one of claims 7-31.
33. The use of the hydrodehydrogenation bidirectional catalytic composition according to any one of claims 1-6 and 32 in organic liquid hydrogen storage.
34. A hydrogenation method, comprising: Under hydrogenation reaction conditions, in the presence of a hydrogenation catalyst, nitrogen-containing heterocyclic organic compounds are brought into contact with hydrogen gas; The hydrogenation catalyst is characterized in that it is the bidirectional catalytic composition for hydrogenation and dehydrogenation as described in any one of claims 1-6 and 32.
35. The hydrogenation method according to claim 34, wherein, The hydrogenation reaction conditions include: a reaction temperature of 50-200℃; and a weight hourly space velocity (WHSV) of 0.5-50 h⁻¹ for nitrogen-containing heterocyclic organic compounds. -1 The hydrogen pressure is 2-10 MPa.
36. The hydrogenation method according to claim 35, wherein, The hydrogenation reaction conditions include: a reaction temperature of 130-200℃; and a weight hourly space velocity of 1-30 h⁻¹ for nitrogen-containing heterocyclic organic compounds. -1 The hydrogen pressure is 5-8 MPa.
37. The hydrogenation method according to any one of claims 34-36, wherein, The nitrogen-containing heterocyclic organic compound is selected from at least one of indole, quinoline, isoquinoline, N-alkylcarbazole, and alkyl-substituted carbazole on the benzene ring.
38. The hydrogenation method according to claim 37, wherein, The alkyl-substituted carbazole on the benzene ring is 2-methylcarbazole and / or 3-methylcarbazole; And / or, the N-alkylcarbazole is N-methylcarbazole and / or N-ethylcarbazole.
39. A dehydrogenation method, comprising: Under dehydrogenation reaction conditions, the hydrogenation products of nitrogen-containing heterocyclic organic compounds are contacted with a dehydrogenation catalyst to carry out a dehydrogenation reaction to obtain hydrogen gas; The dehydrogenation catalyst is characterized in that it is the hydrodehydrogenation bidirectional catalytic composition according to any one of claims 1-6 and 32.
40. The dehydrogenation method according to claim 39, wherein, The dehydrogenation reaction conditions include: a reaction temperature of 100-250℃, and a weight hourly space velocity (WHSV) of 0.5-50 h⁻¹ for the hydrogenation products of nitrogen-containing heterocyclic organic compounds. -1 The reaction pressure is 0.1-2 MPa; And / or, the contact is carried out under hydrogen-exposed or non-hydrogen-exposed conditions; And / or, the nitrogen-containing heterocyclic organic compound is selected from at least one of indole, quinoline, isoquinoline, N-alkylcarbazole, and alkyl-substituted carbazole on a benzene ring.
41. The dehydrogenation method according to claim 40, wherein, The alkyl-substituted carbazole on the benzene ring is 2-methylcarbazole and / or 3-methylcarbazole; And / or, the N-alkylcarbazole is N-methylcarbazole and / or N-ethylcarbazole.
42. The dehydrogenation method according to claim 39, wherein, The hydrogenation product of the nitrogen-containing heterocyclic organic compound is the hydrogenation product of N-ethylcarbazole.
Citation Information
Patent Citations
Organic hydrogen storage material hydrogenation and dehydrogenation catalyst and preparation method thereof
CN110841630A
Preparation method and application of non-noble metal and noble metal bimetallic catalyst for hydrogenation and dehydrogenation of organic hydrogen storage material
CN111569901A
Preparation method of catalyst for ethane oxidative dehydrogenation to ethylene
CN105727978A