加氢催化剂及其制备方法和精制轻质富芳馏分油制BTX的方法

By improving the composition and preparation method of the hydrogenation catalyst, the problem of low catalyst stability was solved, and the efficient conversion of light aromatic-rich distillate oil into BTX was achieved, thereby improving the catalyst stability and BTX yield.

CN117943110BActive Publication Date: 2026-11-24CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211330433.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-27
Publication Date
2026-11-24
Estimated Expiration
2042-10-27

AI Technical Summary

Technical Problem

Existing technologies for processing aromatic cracked distillate oils suffer from low catalyst stability, resulting in low BTX yields and high hydrogen consumption, thus wasting valuable aromatic resources.

Method used

A hydrogenation catalyst comprising Ni, rare earth metal oxides, ZSM-5 and β zeolite was used. It was modified with chelating agents and ascorbic acid, dried in an inert atmosphere and calcined in a low oxygen-content inert atmosphere to reduce the reduction temperature of TPR hydrogen atmosphere and improve the stability of the catalyst.

Benefits of technology

It achieves high stability and high BTX yield, with minimal decrease in catalyst activity over 2000 hours, a total liquid product yield greater than 80%, a BTX yield greater than 55%, and effective utilization of light aromatic-rich distillate oil.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117943110B_ABST
    Figure CN117943110B_ABST
Patent Text Reader

Abstract

This invention relates to the field of hydrotreating, specifically to a hydrotreating catalyst and its preparation method, and a method for producing BTX catalyst from highly stable refined light aromatic-rich distillate oil. The catalyst comprises the following components: a) 5.00%–20.00% Ni; b) 0.01%–5.00% rare earth metal oxides; c) 50.00%–84.99% ZSM-5; d) 5.00%–39.99% β-zeolite; e) 5.00%–20.00% binder; the catalyst carbon deposition is 0.1%–5% of the catalyst weight. The hydrotreating catalyst provided by this invention exhibits high stability and a long operating cycle. The hydrotreating catalyst provided by this invention effectively solves the problem of the inability to utilize refined light aromatic-rich cracked distillate oil for high-value-added production of BTX, enabling the efficient conversion of low-value-added light aromatic-rich cracked distillate oil into high-value-added BTX.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of hydrotreating, specifically to a hydrotreating catalyst and its preparation method, and a method for producing BTX catalyst from highly stable refined light aromatic-rich distillate oil. Background Technology

[0002] Aromatic cracked distillate is a product of high-temperature condensation of feedstock and products during the steam cracking process of ethylene cracking. It mainly comes from the bottom of the quench oil tower and the bottom of the heavy fuel oil stripping tower. Aromatic cracked distillate is a heavy distillate oil (>205℃) rich in aromatics (aromatic content greater than 90%). Its main components are monocyclic and polycyclic aromatic compounds with short side chains, high carbon-hydrogen ratio, and low content of heavy metals and ash. The oil also contains heterocyclic compounds of elements such as N, S, and O.

[0003] The yield of rich aromatic cracked distillate oil is relatively high in the 170℃–300℃ range, followed by very heavy gum and asphaltenes. It also has high sulfur content, high polycyclic aromatic hydrocarbon (PAH) content, and high density. The main components of the initial boiling point to 205℃ range are indene and its homologues; the 205–225℃ range contains naphthalene; the 225–245℃ range is mainly methylnaphthalene; the 245–300℃ range is mainly dimethylnaphthalene; the 300–360℃ range contains large amounts of anthracene, acenaphthene, and phenanthrene; and the substances above 360℃ are mainly gums and asphaltenes with a high C-H ratio; among these, naphthalene-based and higher PAHs account for more than 60%.

[0004] Rich-aromatic cracked distillate oil is mainly used as a raw material for the production of carbon black. Several companies have also begun to use cracked fuel oil to produce aromatic solvent oils, with major manufacturers including ExxonMobil (USA), Shell (Netherlands), and Maruzen Oil Company (Japan).

[0005] Cracked C9 fraction is also a type of aromatic cracked distillate oil, mainly derived from the cracked gasoline C9 fraction separated after passing through the BTX tower. Its aromatic content is as high as 70% or more (more than 90% after extracting dicyclopentadiene), accounting for 11% to 22% of ethylene production.

[0006] How to utilize these low-value-added aromatic-rich cracked distillates is a problem that petrochemical scientists urgently need to solve. Benzene (B), toluene (T), and xylene (X) are important basic organic chemical raw materials, widely used in the production of polyester, chemical fibers, and other products. They are closely related to national economic development and people's basic needs, and demand has been strong and rapidly increasing in recent years. Considering the abundant aromatic resources in ethylene tar and cracked C9, how to convert low-value-added aromatic-rich cracked distillates into BTX through catalytic conversion technology presents both a huge opportunity and a significant challenge.

[0007] In the field of hydrotreating rich aromatic distillate fuels, catalytic cracking feedstock hydrotreating technology has been industrially applied since the 1970s, and has been used in many refineries processing sulfur-containing or high-sulfur crude oils. Currently, mature catalytic cracking feedstock pretreatment technologies include: UOP's VGO Unionfining and APCU (partial conversion hydrocracking) technologies, and Haldor's... The company's Aroshift technology, Chevron's VGO Hydrotreating technology, Exxon's VGO Hydrodesulfurization technology, IFP's T-star technology, and Mobil, AKZO, and Kellogg's MAKfinging technology, among others, are all being utilized. To further improve product quality and conversion rates, catalytic feedstock hydrotreating pretreatment processes are gradually shifting from traditional hydrodesulfurization (HDS) to moderate hydrocracking (MHC) to enhance denitrification, residual carbon, and polycyclic aromatic hydrocarbon saturation capabilities.

[0008] In summary, existing technologies generally employ hydrosaturation and hydrocracking processes. For aromatic-rich cracked distillates with an aromatic content greater than 90%, this not only results in high hydrogen consumption but also wastes valuable aromatic resources. Some technologies, such as CN102234539A, also involve completely saturating the aromatics in the rich aromatic oil before hydrocracking to produce gasoline and diesel, which is costly and uneconomical.

[0009] Based on technologies such as hydrodesulfurization (HDS) and denitrification (HDN) of distillate oil, optimization and innovation are carried out. Through hydrorefining, cracking, alkyl transfer and other means, benzene (B), toluene (T) and xylene (X) can be produced to the maximum extent. The refined light aromatic distillate oil can be fully utilized to increase its added value. Summary of the Invention

[0010] To address the problems of low BTX yield and low catalyst stability in the high-value chemical utilization of refined light aromatic-rich cracked distillate oils in existing technologies, this invention provides a novel hydrogenation catalyst. This hydrogenation catalyst is used for the production of BTX from highly stable refined light aromatic-rich distillate oils and exhibits excellent stability.

[0011] To achieve the aforementioned objective, according to a first aspect of the present invention, a hydrogenation catalyst is provided, the catalyst comprising the following components:

[0012] a)5.00%~20.00%Ni;

[0013] b) 0.01%–5.00% rare earth metal oxides;

[0014] c) 50.00%~84.99% ZSM-5;

[0015] d) 5.00%–39.99% β-zeolite;

[0016] e) 5.00% to 20.00% adhesive;

[0017] The carbon deposition characteristics of the catalyst include: the amount of carbon deposition on the catalyst is 0.1% to 5% of the catalyst weight.

[0018] According to a second aspect of the present invention, the present invention provides a method for preparing the catalyst of the present invention, wherein the method comprises:

[0019] i) Prepare a composite carrier modified with rare earth metal oxides containing ZSM-5, β zeolite and binder;

[0020] ii) Prepare an impregnation solution containing a chelating agent, ascorbic acid, and a Ni source;

[0021] iii) The impregnation solution is impregnated and contacted with the composite carrier, then aged, and then the solid is dried in an inert atmosphere, calcined in a low oxygen inert atmosphere, and then reduced;

[0022] The oxygen content in the low-oxygen inert atmosphere is less than 10% by volume, preferably less than 5% by volume.

[0023] According to a third aspect of the present invention, a method for producing BTX from highly stable refined light aromatic-rich distillate oil is provided. The method comprises: hydrogenating the refined light aromatic-rich cracked distillate oil under hydrogenation reaction conditions in the presence of a catalyst, wherein the catalyst contains the hydrogenation catalyst described in this invention.

[0024] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0025] The hydrogenation catalyst provided by this invention has high stability.

[0026] The method for preparing the hydrogenation catalyst of the present invention involves adding rare earth metals to the support, adding chelating agents and ascorbic acid during the impregnation process, drying in an inert atmosphere, and calcining in a low oxygen-content inert atmosphere. This method simultaneously reduces the hydrogen atmosphere reduction temperature of the catalyst TPR, resulting in a catalyst with strong stability, long catalyst operating cycle, and high BTX yield.

[0027] The hydrogenation catalyst provided by this invention effectively solves the problem of the inability to utilize refined light aromatic cracked distillates at high added value for BTX production. It efficiently converts low-value-added light aromatic cracked distillates into high-value-added BTX. This is suitable for refined light aromatic cracked distillates with an initial boiling point of 85–170℃, a final boiling point of 220–280℃, a total aromatic content greater than 90%, a sulfur content <50ug / mL, and a nitrogen content <10ug / mL. The hydrogenation reaction conditions are: reactor inlet temperature 380–480℃, and fresh feed space velocity 0.6–4.0 h⁻¹. -1 With a hydrogen-to-oil volume ratio of 500–2000 and a pressure of 2–8 MPa, the yield of the initial hydrogenation product in the liquid phase is greater than 80%, and the yield of the liquid phase product BTX is greater than 58%. After 2000 hours of online operation, the catalyst activity decreases little, and the yield of the total liquid phase product is greater than 80%, of which the yield of the liquid phase product BTX is greater than 55%, achieving good technical results. Attached Figure Description

[0028] Figure 1 The XRD patterns of the composite support and hydrogenation catalyst in Example 1 of this invention are shown below.

[0029] Figure 2 Temperature-programmed reduction (TPR) spectrum of the hydrogenation catalyst in Example 1 of this invention;

[0030] Figure 3 The material distribution-online time plot is the evaluation result of the hydrogenation catalyst in Example 1 of this invention;

[0031] Figure 4 The XRD patterns of the composite support and hydrogenation catalyst in Example 2 of this invention are shown below.

[0032] Figure 5 The temperature-programmed reduction (TPR) spectrum of the hydrogenation catalyst in Example 2 of this invention is shown below.

[0033] Figure 6 The temperature-programmed reduction (TPR) spectrum of the catalyst in Comparative Example 1 of this invention is shown below.

[0034] Figure 7 This is a product distribution-online time plot of the evaluation results of Comparative Example 1 of the present invention;

[0035] Figure 8 The temperature-programmed reduction (TPR) spectrum of the catalyst in Comparative Example 2 of this invention is shown. Detailed Implementation

[0036] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0037] This invention provides a hydrogenation catalyst comprising the following components:

[0038] a)5.00%~20.00%Ni;

[0039] b) 0.01%–5.00% rare earth metal oxides;

[0040] c) 50.00%~84.99% ZSM-5;

[0041] d) 5.00%–39.99% β-zeolite;

[0042] e) 5.00% to 20.00% adhesive;

[0043] The amount of carbon deposited on the catalyst is 0.1% to 5% of the catalyst weight. The hydrogenation catalyst provided by this invention exhibits high stability. In this invention, the test method for the carbon deposition characteristics of the catalyst is thermogravimetric analysis.

[0044] According to a preferred embodiment of the present invention, preferably, the dispersion of the active component Ni is greater than 8%, and more preferably 9% to 20%.

[0045] In this invention, all rare earth metals can be used. According to the preferred embodiment of this invention, the rare earth metal is preferably one or more of lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu), and more preferably one or more of cerium, lanthanum, praseodymium, europium, and neodymium.

[0046] In this invention, the range of adhesives that can be selected is relatively wide, and commonly used adhesives can all be used in this invention. For example, the adhesive can be selected from silicon dioxide and / or aluminum oxide.

[0047] According to a preferred embodiment of the present invention, the catalyst contains, by weight percentage, 10% to 15% Ni, 0.01% to 3.0% rare earth metal oxides, 55.00% to 75.50% ZSM-5, 6.00% to 26.50% β zeolite, and 8% to 15% binder.

[0048] According to a preferred embodiment of the present invention, the catalyst contains, by weight percentage, 10% to 15% Ni, 0.01% to 3.0% CeO2, 8% to 15% binder, 55.00% to 75.50% ZSM-5, and 6.00% to 26.50% β-zeolite.

[0049] Catalysts possessing the aforementioned characteristics of this invention can all be used in this invention. There are no special requirements for the catalyst preparation method. For this invention, a preferred catalyst preparation method includes:

[0050] i) Prepare a composite carrier modified with rare earth metal oxides containing ZSM-5, β zeolite and binder;

[0051] ii) Prepare an impregnation solution containing a chelating agent, ascorbic acid, and a Ni source;

[0052] iii) The impregnation solution is impregnated and contacted with the composite carrier, then aged, and then the solid is dried in an inert atmosphere, calcined in a low oxygen inert atmosphere, and then reduced;

[0053] The oxygen content in the low-oxygen inert atmosphere is less than 10% by volume, preferably less than 5% by volume.

[0054] The method for preparing the hydrogenation catalyst of the present invention involves adding rare earth metals to the support, adding chelating agents and ascorbic acid during the impregnation process, drying in an inert atmosphere, and calcining in a low oxygen-content inert atmosphere. This method simultaneously reduces the hydrogen atmosphere reduction temperature of the catalyst TPR, resulting in a catalyst with strong stability, long catalyst operating cycle, and high BTX yield.

[0055] In this invention, the range of selectable conditions for immersion contact is relatively wide. According to a preferred embodiment of this invention, the immersion temperature is 10–80°C.

[0056] The present invention does not have special requirements for the method of immersion contact, and various immersion contact methods can be used. According to a preferred embodiment of the present invention, the composite carrier is immersed by spraying.

[0057] In this invention, aging refers to maintaining the immersion contact for a period of time. According to a preferred embodiment of this invention, the aging time is 0.5 to 24 hours.

[0058] In this invention, the range of drying conditions is relatively wide, and commonly used drying conditions can all be used in this invention. For this invention, the preferred drying temperature is 30 to 200°C.

[0059] In this invention, the range of roasting conditions is relatively wide. The preferred roasting conditions for this invention include a temperature of 300 to 600°C and a roasting time determined as needed. For this invention, the preferred roasting time is 0.5 to 24 hours.

[0060] In this invention, the reduction conditions can be selected from a wide range. The preferred reduction conditions for this invention include: the reduction peak temperature of the catalyst in the TPR hydrogen atmosphere before reduction is below 390°C.

[0061] The reduction temperature of TPR in a hydrogen atmosphere is below 390℃.

[0062] In this invention, the dry inert atmosphere can be any inert gas atmosphere. For this invention, the dry inert atmosphere is preferably one or more of nitrogen atmosphere and argon atmosphere, with nitrogen atmosphere being the most preferred.

[0063] In this invention, the oxygen content in the oxygen-containing inert atmosphere during roasting is preferably 0.1-5% by volume, and the inert gas content is preferably 95-99.9% by volume. Any inert gas can be used in this invention. For this invention, the inert gas is preferably one or more of nitrogen and argon.

[0064] In this invention, the range of chelating agents is relatively wide. For this invention, the preferred chelating agent is selected from one or more of 1-hydroxyethylidene-1,1-diphosphonic acid, tetrasodium hydroxyethylidene diphosphonate (HEDP tetrasodium), aminotrimethylphosphonic acid (ATMPA), and ethylenediaminetetramethylene phosphoric acid (EDTMP), preferably 1-hydroxyethylidene-1,1-diphosphonic acid (HEDPA) and / or tetrasodium hydroxyethylidene diphosphonate (HEDP tetrasodium).

[0065] In this invention, the composition of the impregnation solution can be selected from a wide range. For this invention, it is preferred that the content of the chelating agent in every 100 ml of impregnation solution is 0.01 to 5 grams.

[0066] According to a preferred embodiment of the present invention, the content of ascorbic acid in every 100 ml of impregnation solution is 0.2 to 5 g.

[0067] According to a preferred embodiment of the present invention, the impregnation contact is an equal-volume impregnation contact.

[0068] In this invention, there are no special requirements for the preparation method of the composite carrier. According to a preferred embodiment of this invention, the preparation method of the composite carrier includes:

[0069] (1) Mix the adhesive source, ZSM-5 powder, β zeolite powder and additives evenly to obtain mixture I;

[0070] (2) Add the above mixture I to an acidic aqueous solution, wherein the acidic aqueous solution contains rare earth nitrates; after mixing, shape, dry and calcin.

[0071] According to a preferred embodiment of the present invention, the preparation method of the composite carrier includes: (1) firstly, mixing the binder, ZSM-5 powder, β zeolite powder and additives evenly to obtain mixture I; (2) adding the above mixture I to an acidic aqueous solution containing 1% to 6% by weight, wherein the acidic aqueous solution contains rare earth nitrates, and the weight ratio of mixture I to the acidic aqueous solution is 100:5 to 100:75. After kneading, the mixture is extruded and shaped, dried, and then calcined at 450 to 650°C for 0.5 to 24 hours to obtain the catalyst composite carrier.

[0072] According to a preferred embodiment of the present invention, preferably, the mass ratio of the adhesive, ZSM-5 powder, β-zeolite powder and additives added, based on alumina, is 1:(3-10):(0.4-3.5):(0.1-0.4).

[0073] According to a preferred embodiment of the present invention, preferably, the acidic aqueous solution also contains alkaline earth nitrates. The rare earth nitrates are calculated as rare earth oxides, and the alkaline earth nitrates are calculated as alkaline earth oxides. As a percentage by weight of the acidic aqueous solution, the acidic aqueous solution contains 1%–6% acidic aqueous solution, 1%–5% rare earth oxides, and 1%–2% alkaline earth oxides.

[0074] According to a preferred embodiment of the present invention, the calcination conditions include: a temperature of 450–650°C and a time of 0.5–24 h.

[0075] In this invention, both ZSM-5 powder and β-zeolite powder can be used. For this invention, ZSM-5 powder is preferably in the hydrogen form, and the SiO2 / Al2O3 molar ratio is 50 to 300.

[0076] According to a preferred embodiment of the present invention, the β-zeolite powder is in the hydrogen form, and the SiO2 / Al2O3 molar ratio is 20 to 200.

[0077] In this invention, the range of types of adhesive sources is relatively wide, and commonly used adhesive sources can all be used in this invention. For this invention, the adhesive source is preferably selected from at least one of silica sol, water glass, boehmite, silica, and alumina sol.

[0078] In this invention, the range of selectable adjuvants is relatively wide, and commonly used adjuvants can all be used in this invention. For this invention, the preferred adjuvant is selected from at least one of methylcellulose, fennel powder, polyethylene glycol, calcium nitrate, potassium nitrate, and hydroxymethylcellulose.

[0079] In this invention, the range of types of acidic aqueous solutions is relatively wide, and commonly used acidic aqueous solutions can all be used in this invention. For this invention, it is preferred that the acidic substance in the acidic aqueous solution is selected from at least one of nitric acid, phosphoric acid, acetic acid, citric acid and tartaric acid.

[0080] According to a preferred embodiment of the present invention, the ZSM-5 powder is in the hydrogen form with a SiO2 / Al2O3 ratio of 50 to 300, the β-zeolite powder is in the hydrogen form with a SiO2 / Al2O3 ratio of 20 to 200, the binder is selected from at least one of silica sol, water glass, boehmite, silica, and alumina sol, and the additives are selected from at least one of methylcellulose, tianqing powder, polyethylene glycol, calcium nitrate, potassium nitrate, and hydroxymethylcellulose.

[0081] According to a preferred embodiment of the present invention, the acidic aqueous solution is selected from at least one of nitric acid, phosphoric acid, acetic acid, citric acid, and tartaric acid.

[0082] According to a preferred embodiment of the present invention, an equal-volume impregnation method is used to prepare an impregnation solution by preparing a soluble metal salt precursor containing a required amount of Ni, and adding a chelating agent and ascorbic acid; the amount of chelating agent added is 0.01 to 5% of the weight of the impregnation solution, and the amount of ascorbic acid added is 0.2 to 5% of the weight of the impregnation solution.

[0083] According to a preferred embodiment of the present invention, the catalyst is further prepared by an equal-volume impregnation method at an impregnation temperature of 10–80°C. The catalyst is impregnated onto the composite support by a spray method, and after impregnation, it is left to stand for 0.5–24 hours, dried at 30–200°C, and then calcined at 300–600°C for 0.5–24 hours to obtain the finished catalyst. The TPR hydrogen atmosphere reduction temperature of the catalyst is lower than 390°C, and the dispersion of the active component Ni is greater than 8.0%, preferably 9%–20%.

[0084] According to a preferred embodiment of the present invention, the catalyst of the present invention is further reduced in a hydrogen atmosphere at 200-600°C for 12-72 hours to obtain a reduced catalyst.

[0085] This invention provides a method for producing BTX from highly stable refined light aromatic-rich distillate oil. The method includes: hydrogenating the refined light aromatic-rich cracked distillate oil under hydrogenation reaction conditions in the presence of a catalyst, wherein the catalyst contains the hydrogenation catalyst described in this invention.

[0086] According to a preferred embodiment of the present invention, the refined aromatic light cracked distillate oil has the following characteristics: initial boiling point of 85–170°C, final boiling point of 220–280°C, sulfur content <50 ug / mL, nitrogen content <10 ug / mL, and monocyclic aromatic hydrocarbon content >90 wt%.

[0087] According to a preferred embodiment of the present invention, the hydrogenation reaction conditions include: reactor inlet temperature of 380–480°C and fresh feed space velocity of 0.6–4.0 h⁻¹. -1 The hydrogen-to-oil volume ratio is 500–2000, and the pressure is 2–8 MPa.

[0088] According to a preferred embodiment of the present invention, the refined aromatic light cracked distillate oil has an initial boiling point of 85–170°C and a final boiling point of 220–280°C. The feed composition is: sulfur content <50 ug / mL, nitrogen content <10 ug / mL, and monocyclic aromatic hydrocarbon content >90 wt%. The hydrogenation reaction conditions are: reactor inlet temperature 380–480°C, and fresh feed space velocity 0.6–4.0 h⁻¹. -1 With a hydrogen-to-oil volume ratio of 500–2000 and a pressure of 2–8 MPa, the yield of the total liquid phase product of the initial hydrogenation product is greater than 80%, and the yield of the liquid phase product BTX is greater than 58%.

[0089] According to a preferred embodiment of the present invention, the catalyst operates stably. For refined light aromatic-rich cracked distillate oil with a final boiling point of 220–280°C and a total aromatic content greater than 90%, the catalyst activity decreases by less than 10% after 2000 hours of online operation, and the yield of total liquid products is greater than 80%, of which the yield of liquid product BTX is greater than 55%.

[0090] The present invention will be further illustrated below by way of examples, but these examples are not intended to limit the scope of the present invention.

[0091] In this invention, the dispersion of the active component Ni is tested by hydrogen-oxygen titration.

[0092]

[0093] In the formula: R-----the dispersion of Ni;

[0094] [Ni] ----- Number of nickel atoms on the surface;

[0095] [Ni] 总 -----Total number of nickel atoms;

[0096] V0-----Titration volume of hydrogen, mL;

[0097] N A -----Avogadro's constant (6.023) × 10 23 ;

[0098] W-----Sample mass, g;

[0099] P-----Mass fraction of nickel in the sample, %;

[0100] M-----The atomic weight of nickel is 58.7.

[0101] In this invention, the test method for TPR hydrogen atmosphere reduction is hydrogen-oxygen titration.

[0102] In this invention, the method for calculating the yield of liquid-phase products is as follows:

[0103] Liquid phase product yield = W 液体产物 / W 原料 ,

[0104] W 液体产物 -----Weight of the liquid phase reaction products (in grams) after 24 hours of online processing;

[0105] W 原料 ----Feed amount of refined light aromatic cracked distillate oil feedstock, in grams, for 24-hour online processing.

[0106] In this invention, the reduction peak temperature of the active component Ni is determined using the TPR (temperature-programmed reduction) method. The reduction is carried out in a hydrogen atmosphere, with a heating rate of 10°C / minute, and the temperature is raised to 900°C.

[0107] Carbon deposition was measured using a Multi EA2000 carbon-sulfur analyzer from Jena, Germany. The catalyst was first dried at 150°C for 2 hours, and then tested at a combustion temperature of 900°C with 99.995% pure oxygen as the carrier gas. Spectroscopically pure CaCO3 powder with a carbon mass fraction of 12.00% was used as the standard.

[0108]

Example 1

[0109] 600g of ZSM-5 molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 130, 150g of β molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 40, 100g of boehmite containing alumina, 15g each of methylcellulose and tianqing powder were selected and mixed evenly for later use. Then, 7g of nitric acid and 5g of citric acid were added to 600g of water and dissolved evenly. Cerium nitrate containing 10g of cerium oxide and calcium nitrate containing 8g of calcium oxide were added and dissolved evenly. The solution was poured into the above mixed powder and kneaded for 35 minutes. The mixture was extruded into strips, left to stand for 12 hours, dried at 110℃ for 6 hours, and then calcined in a muffle furnace at 600℃ for 5 hours to obtain the composite carrier with a water absorption rate of 99.1%.

[0110] A soluble metal salt precursor was used to prepare an impregnation solution containing 28 g of Ni, with the solution volume controlled at 170 mL. 1.5 g of 1-hydroxyethylidene-1,1-diphosphonic acid (HEDPA) and 2.0 g of ascorbic acid were added to the impregnation solution and stirred until homogeneous. 172 g of a composite support was then loaded with an equal volume of the impregnation solution using a rotary drum spray method at 40 °C. The mixture was aged for 16 hours, dried at 110 °C for 4 hours in a nitrogen atmosphere, and calcined at 400 °C for 6 hours in a nitrogen atmosphere containing 1.0% oxygen to obtain the catalyst. Reduction at 400 °C in a hydrogen atmosphere for 48 hours yielded the reduced catalyst. The composite support, catalyst preparation conditions, and catalyst carbon deposition are shown in Tables 1, 2, and 3.

[0111] XRD patterns of the composite support and catalyst are shown in [reference needed]. Figure 1, Figure 1 The absence of characteristic peaks for the active component after loading onto the support indicates that the active component has a small particle size and good dispersion on the support; the temperature-programmed reduction (TPR) spectrum of the catalyst is shown below. Figure 2 ,Depend on Figure 2 It can be seen that the peak reduction temperature of the active component under hydrogen atmosphere is 365℃. The dispersion of Ni in the reduced catalyst is 17.6%, indicating that the active component is well dispersed, easy to reduce, and has high catalyst activity.

[0112] Evaluation of raw materials: Refined light aromatic-rich cracking feedstock: distillation range 165-255℃, sulfur content = 0.8ppm, nitrogen content = 0.6ppm;

[0113] Raw material composition: non-aromatic 3.81 wt%; alkylbenzene 40.57 wt%; indene 23.76 wt%;

[0114] Tetrahydronaphthalenes 29.25 wt%; Naphthalenes 2.30 wt%; Benzene 0.31 wt%.

[0115] Reaction conditions: Reactor inlet temperature 410℃, fresh feed space velocity 1.8h. -1 The hydrogen-to-oil volume ratio is 800, and the pressure is 4.0 MPa.

[0116] The evaluation results are shown in Table 4, and the material distribution-online time spectrum of the hydrogenation catalyst is shown in Figure 1. Figure 3 , Figure 3 This indicates that the catalyst has good stability and a high BTX yield.

[0117]

Example 2

[0118] 630 g of ZSM-5 molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 200, 120 g of β molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 20, 100 g of boehmite containing alumina, 15 g each of methylcellulose and tianqing powder were selected and mixed evenly for later use. Then, 7 g of nitric acid and 5 g of citric acid were added to 600 g of water and dissolved evenly. Cerium nitrate containing 10 g of cerium oxide and calcium nitrate containing 8 g of calcium oxide were added and dissolved evenly. The solution was poured into the above mixed powder and kneaded for 35 minutes. The mixture was extruded into strips and left to stand for 12 hours. After drying at 110°C for 6 hours, it was calcined in a muffle furnace at 600°C for 5 hours to obtain the composite carrier with a water absorption rate of 100.3%.

[0119] A soluble metal salt precursor was used to prepare an impregnation solution containing 28 g of Ni, with the solution volume controlled at 170 mL. 1.3 g of 1-hydroxyethylidene-1,1-diphosphonic acid (HEDPA) and 2.5 g of ascorbic acid were added to the impregnation solution and stirred until homogeneous. 172 g of a composite support was then loaded with an equal volume of the impregnation solution using a rotary drum spray method. The impregnation temperature was 60 °C, followed by aging for 16 hours, drying at 110 °C for 4 hours in a nitrogen atmosphere, and calcination at 400 °C for 6 hours in a nitrogen atmosphere containing 2.0% oxygen to obtain the catalyst. Reduction at 400 °C in a hydrogen atmosphere for 48 hours yielded the reduced catalyst. The composite support, catalyst preparation conditions, and catalyst carbon deposition are shown in Tables 1, 2, and 3.

[0120] XRD patterns of the composite support and catalyst are shown in [reference needed]. Figure 4 , Figure 4 The absence of characteristic peaks for the active component after loading onto the support indicates that the active component has a small particle size and good dispersion on the support; the temperature-programmed reduction (TPR) spectrum of the catalyst is shown below. Figure 5 .Depend on Figure 5 It can be seen that the peak reduction temperature of the active component under hydrogen atmosphere is 368℃. The dispersion of Ni in the reduced catalyst is 16.3%, indicating that the active component is well dispersed, easy to reduce, and has high catalyst activity.

[0121] The raw materials and conditions for evaluation were the same as in Example 1, and the evaluation results are shown in Table 4.

[0122]

Example 3

[0123] 600g of ZSM-5 molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 130, 150g of β molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 40, 100g of boehmite containing alumina, 15g each of methylcellulose and tianqing powder were selected and mixed evenly for later use. Then, 7g of nitric acid and 5g of citric acid were added to 600g of water and dissolved evenly. Cerium nitrate containing 10g of cerium oxide and calcium nitrate containing 8g of calcium oxide were added and dissolved evenly. The solution was poured into the above mixed powder and kneaded for 35 minutes. The mixture was extruded into strips, left to stand for 12 hours, dried at 110℃ for 6 hours, and then calcined in a muffle furnace at 600℃ for 5 hours to obtain the composite carrier with a water absorption rate of 99.1%.

[0124] A soluble metal salt precursor was used to prepare an impregnation solution containing 28 g of Ni, with the solution volume controlled at 170 mL. 1.5 g of 1-hydroxyethylidene-1,1-diphosphonic acid (HEDPA) and 9.0 g of ascorbic acid were added to the impregnation solution and stirred until homogeneous. 172 g of a composite support was then loaded with an equal volume of the impregnation solution using a rotary drum spray method at 40 °C. The impregnation was followed by aging at 16 hours, drying at 110 °C for 4 hours in a nitrogen atmosphere, and calcination at 400 °C for 6 hours in a nitrogen atmosphere containing 1.0% oxygen to obtain the catalyst. Reduction at 400 °C in a hydrogen atmosphere for 48 hours yielded the reduced catalyst. The composite support, catalyst preparation conditions, and catalyst carbon deposition are shown in Tables 1, 2, and 3.

[0125] The peak reduction temperature of the active component under a hydrogen atmosphere is 382℃. The dispersion of Ni in the reduced catalyst is 8.7%, indicating that the dispersion of the active component is generally moderate.

[0126] The raw materials and conditions for evaluation were the same as in Example 1, and the evaluation results are shown in Table 4.

[0127]

Example 4

[0128] The method is the same as in Example 1, except that the chelating agent content in the impregnation solution is 0.005% by weight. 600g of ZSM-5 molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 130, 150g of β molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 40, 100g of boehmite containing alumina, 15g each of methylcellulose and tianqing powder are mixed evenly and set aside. Then, 7g of nitric acid and 5g of citric acid are added to 600g of water and dissolved evenly. Cerium nitrate containing 10g of cerium oxide and calcium nitrate containing 8g of calcium oxide are then added and dissolved evenly. The solution is poured into the above mixed powder and kneaded for 35 minutes. The mixture is then extruded into strips, left to stand for 12 hours, dried at 110°C for 6 hours, and then calcined in a muffle furnace at 600°C for 5 hours to obtain the composite carrier, which has a water absorption rate of 99.1%.

[0129] A soluble metal salt precursor was used to prepare an impregnation solution containing 28 g of Ni, with the solution volume controlled at 170 mL. 0.0085 g of 1-hydroxyethylidene-1,1-diphosphonic acid (HEDPA) and 2.0 g of ascorbic acid were added to the impregnation solution and stirred until homogeneous. 172 g of a composite support was then loaded with an equal volume of the impregnation solution using a rotary drum spray method at 40 °C. The mixture was aged for 16 hours, dried at 110 °C for 4 hours in a nitrogen atmosphere, and calcined at 400 °C for 6 hours in a nitrogen atmosphere containing 1.0% oxygen to obtain the catalyst. Reduction at 400 °C in a hydrogen atmosphere for 48 hours yielded the reduced catalyst. The composite support, catalyst preparation conditions, and catalyst carbon deposition are shown in Tables 1, 2, and 3.

[0130] The peak reduction temperature of the active component under a hydrogen atmosphere is 389℃. The dispersion of Ni in the reduced catalyst is 8.9%, indicating that the dispersion of the active component is generally moderate.

[0131] The raw materials and conditions for evaluation were the same as in Example 1, and the evaluation results are shown in Table 4.

[0132]

Example 5

[0133] The method is the same as in Example 1, except that the oxygen content in the oxygen-containing inert atmosphere during calcination is 8% by volume. 600g of ZSM-5 molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 130, 150g of β molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 40, 100g of boehmite containing alumina, 15g each of methylcellulose and tianqing powder are mixed evenly and set aside. Then, 7g of nitric acid and 5g of citric acid are added to 600g of water and dissolved evenly. Cerium nitrate (calculated as 10g of cerium oxide) and calcium nitrate (calculated as 8g of calcium oxide) are added and dissolved evenly. The solution is poured into the above mixed powder and kneaded for 35 minutes. The mixture is then extruded into strips, left to stand for 12 hours, dried at 110°C for 6 hours, and then calcined in a muffle furnace at 600°C for 5 hours to obtain the composite carrier, which has a water absorption rate of 99.1%.

[0134] A soluble metal salt precursor was used to prepare an impregnation solution containing 28 g of Ni, with the solution volume controlled at 170 mL. 1.5 g of 1-hydroxyethylidene-1,1-diphosphonic acid (HEDPA) and 2.0 g of ascorbic acid were added to the impregnation solution and stirred until homogeneous. 172 g of a composite support was then loaded with an equal volume of the impregnation solution using a rotary drum spray method at 40 °C. The mixture was aged for 16 hours, dried at 110 °C for 4 hours in a nitrogen atmosphere, and calcined at 400 °C for 6 hours in a nitrogen atmosphere containing 8.0% oxygen to obtain the catalyst. Reduction at 400 °C in a hydrogen atmosphere for 48 hours yielded the reduced catalyst. The composite support, catalyst preparation conditions, and catalyst carbon deposition are shown in Tables 1, 2, and 3.

[0135] The peak reduction temperature of the active component under a hydrogen atmosphere is 385℃. The dispersion of Ni in the reduced catalyst is 11.6%, indicating that the dispersion of the active component is generally moderate.

[0136] The raw materials and conditions for evaluation were the same as in Example 1, and the evaluation results are shown in Table 4.

[0137]

Example 6

[0138] 600g of ZSM-5 molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 130, 150g of β molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 40, 100g of boehmite containing alumina, 15g each of methylcellulose and tianqing powder were selected and mixed evenly for later use. Then, 7g of nitric acid and 5g of citric acid were added to 600g of water and dissolved evenly. Then, europium nitrate containing 8g of europium oxide and calcium nitrate containing 8g of calcium oxide were added and dissolved evenly. The solution was poured into the above mixed powder and kneaded for 35 minutes. It was then extruded into strips, left to stand for 12 hours, dried at 110℃ for 6 hours, and then calcined in a muffle furnace at 600℃ for 5 hours to obtain the composite carrier with a water absorption rate of 100.1%.

[0139] A soluble metal salt precursor was used to prepare an impregnation solution containing 20 g of Ni, with the solution volume controlled at 180 mL. 6.0 g of 1-hydroxyethylidene-1,1-diphosphonic acid (HEDPA) and 5.0 g of ascorbic acid were added to the impregnation solution and stirred until homogeneous. 180 g of a composite support was then loaded with an equal volume of the impregnation solution using a rotary drum spray method at 40 °C. The impregnation was followed by aging at 16 hours, drying at 110 °C for 4 hours in a nitrogen atmosphere, and calcination at 400 °C for 6 hours in a nitrogen atmosphere containing 1.0% oxygen to obtain the catalyst. Reduction at 400 °C in a hydrogen atmosphere for 48 hours yielded the reduced catalyst. The composite support, catalyst preparation conditions, and catalyst carbon deposition are shown in Tables 1, 2, and 3.

[0140] The peak reduction temperature of the active component under a hydrogen atmosphere was 367℃. The dispersion of Ni in the reduced catalyst was 16.8%, indicating that the active component was well dispersed, easy to reduce, and had high catalyst activity.

[0141] The raw materials and conditions for evaluation were the same as in Example 1, and the evaluation results are shown in Table 4.

[0142]

Example 7

[0143] 600g of ZSM-5 molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 130, 150g of β molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 40, 100g of boehmite containing alumina, 15g each of methylcellulose and Tianqing powder were mixed evenly and set aside. Then, 7g of nitric acid and 5g of citric acid were added to 600g of water and dissolved evenly. Then, lanthanum nitrate containing 10g of lanthanum oxide and calcium nitrate containing 8g of calcium oxide were added and dissolved evenly. The solution was poured into the above mixed powder and kneaded for 35 minutes. It was then extruded into strips, left to stand for 12 hours, dried at 110℃ for 6 hours, and then calcined in a muffle furnace at 600℃ for 5 hours to obtain the composite carrier with a water absorption rate of 99.1%.

[0144] A soluble metal salt precursor was used to prepare an impregnation solution containing 28 g of Ni, with the solution volume controlled at 170 mL. 2.5 g of aminotrimethylphosphonic acid (ATMPA) and 2.0 g of ascorbic acid were added to the impregnation solution and stirred until homogeneous. 172 g of a composite support was then loaded with an equal volume of the impregnation solution using a rotary drum spray method at 40 °C. The mixture was aged for 16 hours, dried at 110 °C for 4 hours in a nitrogen atmosphere, and calcined at 400 °C for 6 hours in a nitrogen atmosphere containing 1.0% oxygen to obtain the catalyst. Reduction at 400 °C in a hydrogen atmosphere for 48 hours yielded the reduced catalyst. The composite support, catalyst preparation conditions, and catalyst carbon deposition are shown in Tables 1, 2, and 3.

[0145] The peak reduction temperature of the active component under a hydrogen atmosphere was 370℃. The dispersion of Ni in the reduced catalyst was 15.3%, indicating that the active component was well dispersed, easy to reduce, and had high catalyst activity.

[0146] The raw materials and conditions for evaluation were the same as in Example 1, and the evaluation results are shown in Table 4.

[0147]

Example 8

[0148] 600g of ZSM-5 molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 130, 150g of β molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 40, 100g of boehmite containing alumina, 15g each of methylcellulose and tianqing powder were selected and mixed evenly for later use. Then, 7g of nitric acid and 5g of citric acid were added to 600g of water and dissolved evenly. Cerium nitrate containing 10g of cerium oxide and calcium nitrate containing 8g of calcium oxide were added and dissolved evenly. The solution was poured into the above mixed powder and kneaded for 35 minutes. The mixture was extruded into strips, left to stand for 12 hours, dried at 110℃ for 6 hours, and then calcined in a muffle furnace at 600℃ for 5 hours to obtain the composite carrier with a water absorption rate of 99.1%.

[0149] A soluble metal salt precursor was used to prepare an impregnation solution containing 28 g of Ni, with the solution volume controlled at 170 mL. 1.5 g of ethylenediaminetetramethylene phosphoric acid (EDTMP) and 2.0 g of ascorbic acid were added to the impregnation solution and stirred until homogeneous. 172 g of a composite support was then loaded with an equal volume of the impregnation solution using a rotary drum spray method at 40 °C. The impregnation was followed by aging at 16 hours, drying at 110 °C for 4 hours in a nitrogen atmosphere, and calcination at 400 °C for 6 hours in a nitrogen atmosphere containing 0.5% oxygen to obtain the catalyst. Reduction at 400 °C in a hydrogen atmosphere for 48 hours yielded the reduced catalyst. The composite support, catalyst preparation conditions, and catalyst carbon deposition are shown in Tables 1, 2, and 3.

[0150] The peak reduction temperature of the active component under a hydrogen atmosphere was 369℃. The dispersion of Ni in the reduced catalyst was 14.8%, indicating that the active component was well dispersed, easy to reduce, and had high catalyst activity.

[0151] The raw materials and conditions for evaluation were the same as in Example 1, and the evaluation results are shown in Table 4.

[0152]

Example 9

[0153] 600g of ZSM-5 molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 130, 150g of β molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 40, 100g of boehmite containing alumina, 15g each of methylcellulose and tianqing powder were selected and mixed evenly for later use. Then, 7g of nitric acid and 5g of citric acid were added to 600g of water and dissolved evenly. Cerium nitrate containing 10g of cerium oxide and calcium nitrate containing 8g of calcium oxide were added and dissolved evenly. The solution was poured into the above mixed powder and kneaded for 35 minutes. The mixture was extruded into strips, left to stand for 12 hours, dried at 110℃ for 6 hours, and then calcined in a muffle furnace at 600℃ for 5 hours to obtain the composite carrier with a water absorption rate of 99.1%.

[0154] A soluble metal salt precursor was used to prepare an impregnation solution containing 28 g of Ni. The solution volume was controlled at 170 mL. 1.5 g of tetrasodium hydroxyethylidene diphosphonate (HEDP tetrasodium) and 2.0 g of ascorbic acid were added to the impregnation solution and stirred until homogeneous. 172 g of a composite support was then loaded with an equal volume of the impregnation solution using a rotary drum spray method. The impregnation temperature was 40 °C, followed by aging for 16 hours, drying at 110 °C for 4 hours in a nitrogen atmosphere, and calcination at 400 °C for 6 hours in a nitrogen atmosphere containing 1.0% oxygen to obtain the catalyst. Reduction at 400 °C in a hydrogen atmosphere for 48 hours yielded the reduced catalyst. The composite support, catalyst preparation conditions, and catalyst carbon deposition are shown in Tables 1, 2, and 3.

[0155] The peak reduction temperature of the active component under a hydrogen atmosphere was 372℃. The dispersion of Ni in the reduced catalyst was 12.9%, indicating that the active component was well dispersed, easy to reduce, and had high catalyst activity.

[0156] The raw materials and conditions for evaluation were the same as in Example 1, and the evaluation results are shown in Table 4.

[0157]

Example 10

[0158] 600g of ZSM-5 molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 130, 150g of β molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 40, 100g of boehmite containing alumina, 15g each of methylcellulose and tianqing powder were selected and mixed evenly for later use. Then, 7g of nitric acid and 5g of citric acid were added to 600g of water and dissolved evenly. Cerium nitrate containing 10g of cerium oxide and calcium nitrate containing 8g of calcium oxide were added and dissolved evenly. The solution was poured into the above mixed powder and kneaded for 35 minutes. The mixture was extruded into strips, left to stand for 12 hours, dried at 110℃ for 6 hours, and then calcined in a muffle furnace at 600℃ for 5 hours to obtain the composite carrier with a water absorption rate of 99.1%.

[0159] A soluble metal salt precursor was used to prepare an impregnation solution containing 28 g of Ni, with the solution volume controlled at 170 mL. 0.75 g of 1-hydroxyethylidene-1,1-diphosphonic acid (HEDPA), 0.75 g of tetrasodium hydroxyethylidene diphosphonate (HEDP tetrasodium), and 2.0 g of ascorbic acid were added to the impregnation solution and stirred until homogeneous. 172 g of a composite support was then loaded with an equal volume of the impregnation solution using a rotary drum spray method at 40 °C. The mixture was aged for 16 hours, dried at 110 °C for 4 hours in a nitrogen atmosphere, and calcined at 400 °C for 6 hours in a nitrogen atmosphere containing 1.0% oxygen to obtain the catalyst. Reduction at 400 °C in a hydrogen atmosphere for 48 hours yielded the reduced catalyst. The composite support, catalyst preparation conditions, and catalyst carbon deposition are shown in Tables 1, 2, and 3.

[0160] The peak reduction temperature of the active component under a hydrogen atmosphere was 366℃. The dispersion of Ni in the reduced catalyst was 16.8%, indicating that the active component was well dispersed, easy to reduce, and had high catalyst activity.

[0161] The raw materials and conditions for evaluation were the same as in Example 1, and the evaluation results are shown in Table 4.

[0162]

Comparative Example 1

[0163] 600g of ZSM-5 molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 130, 150g of β molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 40, 100g of boehmite containing alumina, 15g each of methylcellulose and tianqing powder were selected and mixed evenly for later use. Then, 7g of nitric acid and 5g of citric acid were added to 600g of water and dissolved evenly. Cerium nitrate containing 10g of cerium oxide and calcium nitrate containing 8g of calcium oxide were added and dissolved evenly. The solution was poured into the above mixed powder and kneaded for 35 minutes. The mixture was extruded into strips, left to stand for 12 hours, dried at 110℃ for 6 hours, and then calcined in a muffle furnace at 600℃ for 5 hours to obtain the composite carrier with a water absorption rate of 99.1%.

[0164] A soluble metal salt precursor was used to prepare an impregnation solution containing 28 g of Ni. The solution volume was controlled at 170 mL. 172 g of composite support was used, and an equal volume of the impregnation solution was loaded onto the composite support using a rotary drum spray method. The impregnation temperature was 40 °C, and the mixture was aged for 16 hours. After drying at 110 °C in air for 4 hours, it was calcined at 400 °C for 6 hours to obtain the catalyst. The catalyst was then reduced at 400 °C in a hydrogen atmosphere for 48 hours to obtain the reduced catalyst. The composite support, catalyst preparation conditions, and catalyst carbon deposition are shown in Tables 1, 2, and 3.

[0165] The temperature-programmed reduction (TPR) spectrum of the catalyst is shown below. Figure 6 .Depend on Figure 6 It can be seen that the peak reduction temperature of the active component under hydrogen atmosphere is 415℃. The dispersion of Ni in the reduced catalyst is 4.8%, indicating that the active component has poor dispersion, is difficult to reduce, and has low catalyst activity.

[0166] The evaluation materials and conditions were the same as in Example 1. The evaluation results are shown in Table 4. The material distribution-online time spectrum of the catalyst evaluation results is shown in Table 4. Figure 7 , Figure 7 This indicates that the catalyst's initial activity decreases rapidly and its stability is poor. After 200 hours of online operation, the BTX yield is 53.3%, and after 2000 hours of online operation, the BTX yield decreases to 34.0%.

[0167] [Comparative Example 2]

[0168] 600g of ZSM-5 molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 130, 150g of β molecular sieve powder with a hydrogen form SiO2 / Al2O3 ratio of 40, 100g of boehmite containing alumina, 15g each of methylcellulose and tianqing powder were selected and mixed evenly for later use. Then, 7g of nitric acid and 5g of citric acid were added to 600g of water and dissolved evenly. Cerium nitrate containing 10g of cerium oxide and calcium nitrate containing 8g of calcium oxide were added and dissolved evenly. The solution was poured into the above mixed powder and kneaded for 35 minutes. The mixture was extruded into strips, left to stand for 12 hours, dried at 110℃ for 6 hours, and then calcined in a muffle furnace at 600℃ for 5 hours to obtain the composite carrier with a water absorption rate of 99.1%.

[0169] A soluble metal salt precursor was used to prepare an impregnation solution containing 28 g of Ni, with the solution volume controlled at 170 mL. 1.5 g of 1-hydroxyethylidene-1,1-diphosphonic acid (HEDPA) and 2.0 g of ascorbic acid were added to the impregnation solution and stirred until homogeneous. 172 g of a composite support was then loaded with an equal volume of the impregnation solution using a rotary drum spray method at 40 °C. The impregnation was followed by aging at 16 hours, drying at 110 °C in air for 4 hours, and calcination at 400 °C for 6 hours to obtain the catalyst. Reduction at 400 °C in a hydrogen atmosphere for 48 hours yielded the reduced catalyst. The composite support, catalyst preparation conditions, and catalyst carbon deposition are shown in Tables 1, 2, and 3.

[0170] The temperature-programmed reduction (TPR) spectrum of the catalyst is shown below. Figure 8 ;Depend on Figure 8 It can be seen that the peak reduction temperature of the active component under hydrogen atmosphere is 399℃. The dispersion of Ni in the reduced catalyst is 6.8%, indicating that the active component has poor dispersion, is not easy to reduce, and has low catalyst activity.

[0171] The raw materials and conditions for evaluation were the same as in Example 1, and the evaluation results are shown in Table 4.

[0172] Table 1. Preparation conditions of composite carrier

[0173]

[0174] Table 2 Catalyst preparation conditions, carbon deposition amount, and Ni dispersion

[0175]

[0176]

[0177] As can be seen from the results in Table 2, the catalysts prepared in Examples 1-2 and 6-10 have higher dispersion and lower reduction temperature than those in other examples and comparative examples. Obviously, the catalysts prepared by the method of the present invention have the effects of high dispersion and low reduction temperature.

[0178] Table 3. Amounts of catalyst chelating agent and ascorbic acid added.

[0179]

[0180] Table 4 Catalyst Evaluation Results

[0181]

[0182]

[0183] As shown in Table 4, in Examples 1-2 and 6-10, after 200 hours of online operation, the total liquid product yield was greater than 80%, and the BTX yield was greater than 58%. After 2000 hours of online operation, the total liquid product yield was still greater than 80%, with the BTX yield exceeding 55%, demonstrating good technical performance. In contrast, the BTX yields in Comparative Examples 1 and 2 were 53.3% and 54.2% respectively after 200 hours of online operation; after 2000 hours, the BTX yields were only 34.0% and 40.3% respectively. Clearly, the catalyst provided by this invention exhibits good stability and high BTX yield.

[0184] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A hydrogenation catalyst, characterized in that, The catalyst comprises the following components by weight percentage: a) 5.00%~20.00% Ni; b) 0.01%~5.00% rare earth metal oxides; c) 50.00%~84.99% ZSM-5; d) 5.00%~39.99% β-zeolite; e) 5.00%~20.00% adhesive; The amount of carbon deposited on the catalyst is 0.1% to 5% of the catalyst weight; The dispersion of the active component Ni is greater than 8%; The adhesive is selected from silica and / or alumina; The method for preparing the catalyst includes: i) Preparation of rare earth metal oxide modified composite carriers containing ZSM-5, β-zeolite and binder; ii) Prepare an impregnation solution containing a chelating agent, ascorbic acid, and a Ni source; iii) The impregnation solution is impregnated and contacted with the composite carrier, then aged, and then the solid is dried in an inert atmosphere, calcined in a low oxygen inert atmosphere, and then reduced; The oxygen content in the low-oxygen inert atmosphere is less than 10% by volume.

2. The catalyst according to claim 1, wherein, The dispersion of the active component Ni is 9%~20%; and / or Rare earth metals are one or more of the following: lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium. and / or The catalyst contains, by weight percentage, 10% to 15% Ni, 0.01% to 3.0% rare earth metal oxides, 55.00% to 75.50% ZSM-5, 6.00% to 26.50% β zeolite, and 8% to 15% binder.

3. The catalyst according to claim 1, wherein, Rare earth metals are one or more of cerium, lanthanum, praseodymium, europium, and neodymium.

4. The catalyst according to any one of claims 1-3, wherein, The oxygen content in the low-oxygen inert atmosphere is below 5% by volume.

5. The catalyst according to any one of claims 1-3, wherein, Step iii). Conditions for immersion contact include: The impregnation temperature is 10~80℃; and / or The composite carrier is impregnated by spraying; and / or The aging time is 0.5~24 hours.

6. The catalyst according to any one of claims 1-3, wherein, Step iii). Drying conditions include: a temperature of 30~200℃; and / or The roasting conditions include: a temperature of 300~600℃, and / or a time of 0.5~24h; and / or The TPR reduction peak temperature of the catalyst before reduction is below 390℃ in a hydrogen atmosphere.

7. The catalyst according to any one of claims 1-3, wherein, The dry, inert atmosphere is one or more of nitrogen and argon; and / or The oxygen content in the oxygen-containing inert atmosphere during roasting is 0.1-5% by volume, and the inert gas content is 95-99.9% by volume.

8. The catalyst according to claim 7, wherein, The dry, inert atmosphere is a nitrogen atmosphere; and / or The inert gas in the oxygen-containing inert atmosphere during roasting is one or more of nitrogen and argon.

9. The catalyst according to any one of claims 1-3, wherein, The chelating agent is selected from one or more of 1-hydroxyethylidene-1,1-diphosphonic acid, tetrasodium hydroxyethylidene diphosphonate, aminotrimethylphosphonic acid, and ethylenediaminetetramethylene phosphoric acid; and / or The chelating agent content is 0.01~5 g per 100 ml of impregnation solution; and / or The ascorbic acid content is 0.2-5 grams per 100 ml of impregnation solution; and / or The impregnation contact is an equal-volume impregnation contact.

10. The catalyst according to any one of claims 1-3, wherein, The chelating agent is selected from 1-hydroxyethylidene-1,1-diphosphonic acid and / or tetrasodium hydroxyethylidene diphosphonate.

11. The catalyst according to any one of claims 1-3, wherein, Methods for preparing composite supports include: (1) Mix the binder source, ZSM-5 powder, β zeolite powder and additives evenly to obtain mixture I; (2) Add the above mixture I to an acidic aqueous solution, wherein the acidic aqueous solution contains rare earth nitrates; after mixing, shape, dry and calcin.

12. The catalyst according to claim 11, wherein, The concentration of acidic substances in the acidic aqueous solution is 1% to 6% by weight. and / or The weight ratio of mixture I to the acidic aqueous solution is 100:5 to 100:75; and / or The roasting conditions include a temperature of 450~650℃ and a time of 0.5~24h.

13. The catalyst according to claim 11, wherein, ZSM-5 powder is in the hydrogen form, with a SiO2 / Al2O3 molar ratio of 50~300; and / or β-zeolite powder is in the hydrogen form, with a SiO2 / Al2O3 molar ratio of 20~200; and / or The binder source is selected from at least one of silica sol, water glass, boehmite, silica, and alumina sol; and / or The additives are selected from at least one of methylcellulose, fennel powder, polyethylene glycol, calcium nitrate, potassium nitrate, and hydroxymethylcellulose; The acidic substance in the acidic aqueous solution is selected from at least one of nitric acid, phosphoric acid, acetic acid, citric acid and tartaric acid.

14. A method for producing BTX from highly stable refined light aromatic-rich distillate oil, characterized in that, The method includes: In the presence of a catalyst and under hydrogenation reaction conditions, refined aromatic light cracked distillate oil is hydrogenated, wherein the catalyst is the catalyst described in any one of claims 1-13.

15. The method according to claim 14, wherein, Refined aromatic light cracked distillate oil: initial boiling point 85~170℃, final boiling point 220~280℃, sulfur content <50ug / mL, nitrogen content <10ug / mL; monocyclic aromatic hydrocarbon content >90wt%; The hydrogenation reaction conditions include: reactor inlet temperature 380~480℃, and fresh feed space velocity 0.6~4.0 h⁻¹. -1 The hydrogen-to-oil volume ratio is 500-2000, and the pressure is 2-8 MPa.

Citation Information

Patent Citations

  • Method for processing ethylene tar

    CN102234539A

  • Hydrodesulfurization catalyst, and preparation method and application thereof

    CN110404527A

  • Method for producing benzene by lightening aromatic-rich distillate oil

    CN115141652A