Carbon sequestration low-calcium cementitious material and method of making
By using municipal solid waste incineration residue to prepare low-calcium cementitious materials based on β-C₂S, and combining this with CO₂ curing to activate the activity, the problems of high carbon emissions and low β-C₂S activity in cement production have been solved, achieving low-carbon production and strength improvement, as well as resource utilization and environmental benefits.
Patent Information
- Application Number
- CN202410094362.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-23
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-01-23
AI Technical Summary
Existing cement production processes suffer from high carbon emissions, high energy consumption, and high costs. In particular, the high calcium mineral composition of traditional cement clinker leads to the consumption of large amounts of carbonate raw materials and the emission of greenhouse gases. At the same time, the low hydration activity of β-C₂S limits its widespread application in cement-based materials.
Using municipal solid waste incineration residue (washed fly ash and bottom ash) as raw materials, low-calcium cementitious materials with β-C₂S as the main component are prepared by low-temperature calcination (1000~1200℃). High-concentration CO₂ curing is used to activate mineral activity, combined with carbonization curing process, to achieve carbon reduction at the source and carbon reduction in the process.
It has achieved low-carbon cement production, reduced calcination energy consumption and costs, improved the later strength of cementitious materials, sealed CO₂, and reduced the overall carbon emissions and harmful gas emissions of cement production, and realized the resource utilization of urban domestic waste.
Smart Images

Figure CN117945675B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of new materials technology, specifically relating to a novel carbon-fixing low-calcium cementitious material and its preparation method. Background Technology
[0002] The cement industry, as a significant source of industrial CO2 emissions, emitted 1.345 billion tons of CO2 in China in 2021, accounting for approximately 13% of the country's total carbon emissions, second only to the power industry (40%) and the steel industry (14%). Promoting carbon emission reduction in the cement industry is therefore imperative.
[0003] The high carbon footprint of cement production primarily stems from the high-temperature formation (1450℃) of clinker minerals (C3S) and the decomposition of carbonates in limestone, which is attributable to the compositional design of high-calcium minerals in clinker. Furthermore, high-calcium minerals also lead to the excessive consumption of high-quality limestone and coal resources, as well as the generation of greenhouse gases CO2 and harmful gases SO2 and NO. x The large-scale emissions of cement, etc., have exacerbated the energy and resource consumption and environmental burden of the cement industry. Therefore, the most feasible technical solutions to achieve low-carbon production in the cement industry from the source are: (1) Low carbon at the source: using non-carbonate industrial solid waste to replace natural limestone raw materials; (2) Carbon reduction in the process: breaking through the traditional silicate cement clinker system and replacing high-calcium mineral C3S phase with low-calcium minerals; (3) Carbon removal at the end: developing carbon capture and utilization (CCUS) technology to recover and seal carbon emissions in cement production.
[0004] Patent CN 105347706 A discloses a method for preparing self-pulverizing low-calcium cement and its pre-forms, wherein the cement is mainly composed of 30-45% C3S2, 45-65% α-CS, and 5-10% f-CaO; Patent CN 111393051 A invented a grinding-free carbonization hardening cement clinker and its preparation method, wherein the cement clinker incorporates the limiting component f-CaO into its mineral composition, and achieves self-pulverization of the clinker through cooling expansion; Patent CN 111393050 A discloses a method for preparing γ-C2S-based cementitious materials, wherein the cementitious materials are mainly composed of γ-C2S and contain small amounts of β-C2S and C3S2; Although the above methods reduce carbon emissions and grinding power consumption in the cement production process to some extent, they still use natural raw materials such as limestone, sandstone, and iron ore, resulting in high preparation costs and making large-scale industrial production impossible; Patent CN 111393049 A discloses an activation modification method for γ-C2S, which improves carbonization activity by adding metal ions and increasing the specific surface area of γ-C2S. However, this method is complex and costly, and the activation modification does not have a significant effect on the later strength, which can easily lead to problems such as unstable strength development in the later stage.
[0005] Patents CN110475756 A and CN 110475756 B disclose a carbonation-activated clinker binder from incineration residue, said clinker being sintered at 1000–1100°C and containing one or a combination of CO2-reactive mineral components, such as Ca. 10 (SiO4)3(SO4)3Cl2, C2S, CS; also contains the uncarbonized phase Ca6Al5Si2O 16 Cl3 / Ca 12 Al 14 O 33 , Ca8Mg(SiO4)4Cl2, Ca2MgSi2O7 / CaAl2Si2O7, (Ca, Ba) 13 Ingredients include Mg2(SiO4)8, CaSO4, SiO2, and NaCl / KCl. However, during the preparation of this binder, the accumulation of chlorides can easily lead to cement kiln crusting and erosion of refractory materials inside the kiln.
[0006] To address the shortcomings of existing technologies, a method for preparing a product using β-C2S and... (The sentence is incomplete and requires more context to translate accurately.) This novel low-carbon cementitious material, primarily composed of belite (β-C2S), enables low-carbon production in the cement industry and facilitates the co-processing of cement kilns and municipal solid waste. Compared to traditional mineral C3S, belite (β-C2S) and calcium sulfosilicate... The CaO contents were 65.1% and 58.33%, respectively. β-C₂S could be rapidly formed at temperatures above 1250℃. Formed by the reaction of belite and anhydrite at 1150–1250℃, both exhibit advantages in energy conservation and carbon reduction, particularly in terms of natural energy consumption and calcination energy consumption. Based on comprehensive carbon emissions, C2S and... The values are 511 and 458 kg / t respectively (less than C3S, 579 kg / t). Furthermore, It has a relatively rich composition, which can maximize the utilization rate of industrial solid waste.
[0007] However, the hydration activity of β-C2S (especially in the early stages) is very low, only about 1 / 20 of that of the C3S phase. Although researchers have used methods such as thermal activation, ion doping, rapid cooling, and mechanical polishing to improve the hydration activity of β-C2S, the early strength development is still insufficient to meet the requirements of practical engineering. It has always been considered an inert mineral with extremely poor hydration activity, although in Al(OH)4 -While it can be activated by the dissolution of sulfates, the reaction rate remains low, severely limiting its widespread application in cement-based materials. In recent years, the development of CCUS technology has overcome this limitation. It breaks through the traditional approach that cement hardening should not solely rely on cement hydration as a criterion for judging the rationality of mineral composition. By replacing traditional water curing with high-concentration CO2 curing, it not only stimulates the reactivity of these two minerals, reacting with calcium-rich minerals to form stable carbonates, but also absorbs and seals 25-30% CO2, resulting in significant economic and environmental benefits. Summary of the Invention
[0008] In response to the high carbon footprint of the cement industry, this invention aims to provide a novel carbon-fixing, low-calcium cementitious material and its preparation method. It utilizes non-carbonate raw materials—municipal solid waste incineration residue (washed fly ash and bottom ash)—at 1000–1200℃ to prepare materials with β-C₂S and... The low-calcium cementitious material with calcium as its main component solves the problems of high preparation cost, high calcination energy consumption, and slow strength development in the later stage of existing carbonization hardening cementitious materials. It also absorbs and stores 25-30% CO2, resulting in significant economic and environmental benefits. At the same time, it enables the co-processing of municipal solid waste and cement kilns. Through the concept of "carbon reduction at the source, carbon reduction in the process, and carbon removal at the end", it fundamentally realizes low-carbon production in the cement industry.
[0009] To achieve the above objectives, the present invention adopts the following technical solution:
[0010] The aforementioned novel carbon-fixing, low-calcium cementitious material is prepared by the following steps:
[0011] Step 1: Grind, homogenize, and press 61-80 parts of water-washed municipal solid waste incineration fly ash and 20-39 parts of municipal solid waste incineration bottom ash into a cake to obtain a raw material cake for preparing a cementitious material.
[0012] Step 2: The raw material cake obtained in Step 1 is pre-fired and calcined, then cooled and ground to prepare a new type of carbon-fixing low-calcium cementitious material.
[0013] Step 3: Press the gelling material prepared in Step 2 into shape, place it in a pressure reactor or carbonization box for curing for 2-24 hours, and then continue to place it in a standard curing box (T=20±5℃, RH≥90%) until the specified age.
[0014] According to the above scheme, the municipal solid waste incineration fly ash mentioned in step one includes the following components: Ca(OH)2, CaSO4, CaCO3, CaClOH, NaCl and KCl, with a CaO content of 35-60 wt%.
[0015] According to the above scheme, the bottom ash of municipal solid waste incineration in step one includes the following components: SiO2 and CaCO3, with SiO2 content of 55-65 wt%.
[0016] According to the above scheme, the water washing process in step one involves controlling the liquid-to-solid ratio (5, 10, 15, 20), stirring rate (1000, 1500, 2000 r / min), and stirring time (20, 30, 40 min). After sedimentation, filtration (45 μm), and drying, the chlorine content is 0.5-1.3%.
[0017] According to the above scheme, the grinding process in step one is as follows: ball milling at a speed of 450 r / min for 10 to 30 minutes, and the fineness is less than 10% of the residue on an 80 μm square hole sieve.
[0018] According to the above scheme, the homogenization process in step one is as follows: first, the mixture is oscillated for 10 minutes using a high-speed oscillator, and then rotated in an empty ball mill jar (with steel balls removed) at a speed of 250 r / min for 20 to 30 minutes to ensure that the raw materials are fully mixed.
[0019] According to the above scheme, the preparation process of the raw material cake in step one is as follows: 34-38g of mixed semi-dry material is pressed into cake under a pressure of 5-10MPa. (±2) round cake sample.
[0020] According to the above scheme, the pre-firing temperature in step two is 800-950℃, the pre-firing time is 1-2h; the calcination temperature is 1000-1200℃, the calcination time is 1-3h, and the heating rate is 5-10℃ / min.
[0021] According to the above scheme, the grinding process in step two involves ball milling at a speed of 450 r / min for 10–30 min, achieving a fineness of less than 10% residue on an 80 μm square-hole sieve or a specific surface area of 350–450 m². 2 / kg.
[0022] According to the above scheme, the novel carbon-fixing low-calcium cementitious material described in step two, expressed in parts by weight, mainly includes the following mineral phases: β-C2S: 29.8–38.9 parts; 12.7–28.3 parts, Ca2Al2SiO7: 9.1–16.1 parts, Ca 12 Al 14 O 33 : 4.7-7.3 parts, Ca2MgSi2O7: 2.5-6.3 parts, amorphous phase: 13.7-23.9 parts.
[0023] According to the above scheme, the pressing process in step three involves controlling the water-to-solid ratio between 0.1 and 0.18 and holding the pressure at 10 MPa for 25 to 30 seconds.
[0024] According to the above scheme, the curing conditions in the pressurized reactor or carbonization box in step three are: CO2 pressure 0.1-0.5 MPa, concentration 10-99%, temperature 20-60℃; CO2 concentration 20%, temperature 20℃, humidity 65%.
[0025] Compared with existing technologies, the novel carbon-fixing low-calcium cementitious material and its preparation method described in this invention have the following advantages:
[0026] (1) The cementitious material of the present invention uses non-carbonate raw materials—washed fly ash and bottom ash from municipal solid waste incineration as raw materials, and has a low calcination temperature (1000-1200℃). Compared with ordinary silicate cement, it can save 60-100% of natural resources such as limestone and clay, reduce coal consumption by 15-30%, reduce carbon emissions caused by fuel combustion by more than 30%, and reduce carbon emissions caused by decomposition of carbonate raw materials by more than 90%.
[0027] (2) The cementitious material of this invention contains 29.8-38.9% β-C2S (possessing carbonization and slow hydration activity) and 12.7-28.3% β-C2S. (Possessing only carbonization activity), the continuous hydration of this mineral can steadily improve the later strength of cement, and improve the density and strength of carbonized hardened cementitious materials from the source. Compared with methods such as significantly increasing CO2 pressure and adding metal ion compounds, the cost is lower and the process is simpler.
[0028] (3) The cementitious material of this invention is mainly carbonized in the early stage, which not only stimulates the activity of minerals, but also can seal 250-300kg CO2 per ton of cementitious material, reducing the overall carbon emissions of cement production by more than 60%, and the content of alkaline substances such as f-MgO and f-CaO is not strictly controlled. Attached Figure Description
[0029] Figure 1 To implement the mineral phase composition of the clinker sintered at 1000–1200℃ in Section 1;
[0030] Figure 2 To implement the strength of clinker carbonized at 1000-1200℃ for 2h, 6h, and 1d in Section 1;
[0031] Figure 3 To measure the strength of clinker with a calcium-silicon ratio of 2.0 to 4.2 in Example 2 after carbonization at 1000-1200℃ for 1 day. Detailed Implementation
[0032] To better understand the present invention, the present invention will be further described below with reference to specific examples. Obviously, the described embodiments are only preferred embodiments of the present invention and are not intended to limit the present invention.
[0033] The low-calcium cementitious material of this invention is made entirely from municipal solid waste incineration ash (washed fly ash and bottom ash), prepared after calcination and cooling. The firing temperature is 250-450℃ lower than that of traditional silicate cement, saving 60-100% of natural resources such as limestone and clay, reducing coal consumption by 15-30%, and decreasing carbon emissions from fuel combustion by over 30% and carbon emissions from carbonate raw material decomposition by over 90%. Furthermore, it significantly reduces cement production costs and reduces CO2 and harmful gases such as SO2 and NO. x The emission of polluting gases.
[0034] Example 1
[0035] This invention provides a novel carbon-fixing, low-calcium cementitious material and its preparation method, comprising the following steps:
[0036] Step 1, Washing fly ash: Under the conditions of liquid-to-solid ratio of 10 and magnetic stirring speed of 1500r / min, stir for 30min, let stand, settle until solid-liquid separation, filter (45μm), dry, and grind, and then use it as raw material for preparing cementitious materials.
[0037] Step 2, Clinker Calcination: Following a calcium-to-silicon ratio of 3.0, 72 parts of washed fly ash and 28 parts of incinerator bottom ash are mixed in a ball mill at 450 rpm for 15 minutes. The water-to-solid ratio is controlled at 0.1. 36g of the mixture is then pressed at 10MPa for 20 seconds to produce clinker. The round cakes were dried in an 85℃ drying oven to constant weight. They were then pre-calcined in a 950℃ muffle furnace at a heating rate of 10℃ / min for 1 hour, and then calcined at the same rate to 1000-1200℃ for 2 hours. After cooling in the furnace, they were ball-milled at 450r / min for 20 minutes to obtain a novel carbon-fixing low-calcium cementitious material.
[0038] Step 3, Carbonation Curing: Take 87 parts of the cementitious material obtained in Step 2, add 13 parts of deionized water, stir evenly, and press it into 20*20*20mm cubic specimens under a pressure of 10MPa for 30s. Place them in a carbonation chamber (CO2 concentration 20%, temperature 20℃, humidity 65%) for curing for 2h, 6h, and 24h. For comparison, 425 grade Portland cement (OPC) was used as the control group, and its molding and carbonation curing processes were the same as the experimental group.
[0039] The novel carbon-fixed low-calcium cementitious material in this embodiment was subjected to X-ray diffraction testing. After carbonization curing to a fixed age, the mechanical properties of the carbonized product were tested in accordance with JGJ / T70-2009 "Standard for Test Methods of Basic Performance of Building Mortar".
[0040] Tests showed that the clinker sintered at 1000–1200℃ contained the following minerals by mass percentage: 29.8–38.9% β-C₂S, 12.7–28.3% β-C₂S, and 12.7–28.3% β-C₂S. 9.1~16.1% Ca2Al2SiO7, 4.7~7.3% Ca 12 Al 14 O 33 2.5–5.6% Ca2MgSi2O7 and 13.7–23.9% amorphous phase, such as Figure 1 As shown. After clinker sintered at 1000–1200℃ was pressed into shape using the above process and then cured in a carbonization box (CO2 concentration 20%, temperature 20℃, humidity 65%) for 2h, 6h, and 24h respectively, the compressive strengths were 9.4 / 11.7 / 87.8MPa, 9.0 / 15.1 / 103.4MPa, 14.7 / 36.0 / 109.8MPa, 30.4 / 66.0 / 113.9MPa, and 24.5 / 58.8 / 112.6MPa. The strength after 1 day of carbonization was superior to that of OPC. Figure 2 As shown.
[0041] Example 2
[0042] A novel carbon-fixing low-calcium cementitious material and its preparation method, comprising the following steps:
[0043] Step 1, Washing fly ash: Under the conditions of liquid-to-solid ratio of 10 and magnetic stirring speed of 1500r / min, stir for 30min, let stand, settle until solid-liquid separation, filter (45μm), dry, and grind, and then use it as raw material for preparing cementitious materials.
[0044] Step 2, Clinker Calcination: Mix 61-80 parts of washed fly ash and 20-39 parts of incinerator bottom ash in a ball mill at 450 rpm for 15 minutes, maintaining a calcium-to-silicon ratio of 2.0-4.2. Control the water-to-solid ratio at 0.1, and hold 36g of the mixture under 10MPa pressure for 20 seconds to produce clinker. The round cakes were dried in an 85℃ drying oven to constant weight. They were then pre-calcined in a 950℃ muffle furnace at a heating rate of 10℃ / min for 1 hour, and then calcined at the same rate to 1000-1200℃ for 2 hours. After cooling in the furnace, they were ball-milled at 450r / min for 20 minutes to obtain a novel carbon-fixing low-calcium cementitious material.
[0045] Step 3, Carbonization Curing: Take 87 parts of the cementitious material obtained in Step 2, add 13 parts of deionized water, stir evenly, and press it into 20*20*20mm cubic test blocks under a pressure of 10MPa for 30s. Place them in a carbonization chamber (CO2 concentration 20%, temperature 20℃, humidity 65%) for 24 hours of curing. OPC serves as a control group, and the carbonization curing process is the same.
[0046] The novel carbon-fixed low-calcium cementitious material in this embodiment was carbonized and cured for 1 day, and the mechanical properties of the carbonized product were tested in accordance with JGJ / T70-2009 "Standard for Test Methods of Basic Performance of Building Mortar".
[0047] Tests showed that the 1-day strength of clinker sintered at 1100–1200℃ for mixtures with a calcium-silicon ratio of 2.0–4.2 exceeded that of OPC. Among these, the 1-day strength of the clinker sintered at 1100–1200℃ for mixtures with a calcium-silicon ratio of 2.6–3.0 exceeded 100 MPa, significantly higher than the carbonized mechanical properties of OPC. Figure 3 As shown.
Claims
1. A method for preparing a carbon-fixed, low-calcium cementitious material, characterized in that, Includes the following steps: Step 1: According to the calcium-silicon ratio of 2.0~4.2, 61~80 parts of water-washed municipal solid waste incineration fly ash and 20~39 parts of municipal solid waste incineration bottom ash are ground, homogenized and pressed into cakes to obtain raw material cakes for preparing cementitious materials; Step 2: Pre-calcinate and calcine the raw material cake obtained in Step 1; the pre-calcination temperature is 800–950℃, and the pre-calcination time is 1–2 hours; the calcination temperature is 1000–1200℃, and the calcination time is 1–3 hours, with a heating rate of 5–10℃ / min; then cool and grind to prepare a carbon-fixed low-calcium cementitious material, whose main mineral phases, expressed in parts by weight, include: β-C2S: 29.8–38.9 parts, : 12.7~28.3 parts, Ca2Al2SiO7: 9.1~16.1 parts, Ca 12 Al 14 O 33 : 4.7–7.3 parts; Ca2MgSi2O7: 2.5–6.3 parts; amorphous phase: 13.7–23.9 parts; Step 3: Press the carbon-fixed low-calcium cementitious material prepared in Step 2 into shape, place it in a pressure reactor or carbonization box for 2-24 hours, and then continue to place it in a standard curing box until the specified age.
2. The method for preparing a carbon-fixed low-calcium cementitious material according to claim 1, characterized in that, The municipal solid waste incineration fly ash mentioned in step one includes the following components: Ca(OH)2, CaSO4, CaCO3, CaClOH, NaCl and KCl, with a CaO content of 35-60 wt%.
3. The method for preparing a carbon-fixed low-calcium cementitious material according to claim 1, characterized in that, The municipal solid waste incineration bottom ash mentioned in step one includes the following components: SiO2 and CaCO3, with SiO2 content of 55-65 wt%.
4. The method for preparing a carbon-fixing low-calcium cementitious material according to claim 1, characterized in that, The water washing process described in step one involves controlling the liquid-to-solid ratio at 10, the stirring rate at 1500 r / min, and the stirring time at 30 min. After sedimentation, 45 μm filtration, and drying, the chlorine content is 0.5–1.3%.
5. The method for preparing a carbon-fixed low-calcium cementitious material according to claim 1, characterized in that, The fineness of the powder in step one is less than 80 μm.
6. The method for preparing a carbon-fixed low-calcium cementitious material according to claim 1, characterized in that, The preparation process of the raw material cake described in step one: 34-38g of mixed semi-dry material is pressed into cake under a pressure of 5-10MPa. The round cake sample.
7. The method for preparing a carbon-fixed low-calcium cementitious material according to claim 1, characterized in that, In step two, the fineness of the carbon-fixing low-calcium cementitious material prepared by grinding is less than 80 μm or the specific surface area is 350–450 m². 2 / kg.
8. The method for preparing a carbon-fixed low-calcium cementitious material according to claim 1, characterized in that, The pressing process described in step three is as follows: control the water-to-solid ratio between 0.1 and 0.18, and hold the pressure at 10 MPa for 25 to 30 seconds.
Citation Information
Patent Citations
Autogenously-pulverizable low calcium cement, and making method of prefabricated products thereof
CN105347706A
Carbonation-activated clinker binder from incineration residues
CN110475756A
Carbonation-activated clinker binder from incineration residue
CN110475756B