Process for the pre-hydrogenation of acetylene
A catalyst was prepared by supporting palladium on a graphene-coated nanodiamond and an inorganic oxide composite support, which solved the problem of alkyne removal at high temperatures in existing catalysts and achieved efficient selective hydrogenation of acetylene to ethylene at low temperatures, making it suitable for industrial applications.
Patent Information
- Application Number
- CN202211316850.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-26
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-10-26
AI Technical Summary
Existing acetylene pre-hydrogenation catalysts can only achieve complete removal of alkynes under high temperature conditions, which cannot meet the actual needs of industrial applications, and the selectivity is low.
A highly efficient acetylene pre-hydrogenation catalyst was prepared by using graphene-coated nanodiamonds with inorganic oxides, diatomaceous earth, or molecular sieves as composite supports, and loading palladium as the active component. This catalyst is suitable for the selective hydrogenation of acetylene to ethylene under low-temperature conditions.
The catalyst improves the conversion rate and selectivity of selective hydrogenation of acetylene to ethylene, and still has good catalytic effect at low temperature, making it suitable for industrial production.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of selective hydrogenation technology for unsaturated hydrocarbons, and more specifically, to a method for the pre-hydrogenation reaction of acetylene. Background Technology
[0002] Thermocracking of naphtha feedstocks is currently the main method for producing olefins such as ethylene and propylene. While obtaining olefins, the cracking products contain small amounts of alkynes and dienes. The enrichment of these byproducts during separation can pose safety hazards to the production unit. They need to be eliminated sequentially through separation and hydrogenation to meet the requirements of polymerization feedstocks, while also increasing ethylene production and improving resource utilization. Traditional production processes employ sequential separation, where hydrogen, C2, and C3 fractions are separated from the cracking products in sequence, and then alkynes and dienes in each fraction are hydrogenated to remove them. In recent years, pre-hydrogenation separation processes have become more common, where impurity gases such as alkynes and dienes are first hydrogenated before further separation. In this process, the hydrogen content is often as high as 10% or more, and the reaction space velocity is as high as 12000 h⁻¹. -1 Therefore, the catalyst used must not only satisfy the removal of alkynes and dienes, but also have high selectivity, so as to reduce the loss caused by hydrogenating olefins to alkanes under high hydrogen concentration conditions.
[0003] Industrially used selective hydrogenation catalysts for unsaturated alkynes and dienes are mostly supported metal catalysts, generally composed of a support, a main active component, and a co-active component. Commonly used supports include alumina, silica, molecular sieves, activated carbon, magnesium oxide, titanium oxide, diatomaceous earth, etc. The main active component is a metal element with hydrogenation catalytic activity, usually a Group VIII element, such as Pd, Pt, Ni, etc., with Pd being the most commonly used selective hydrogenation active component. Although the catalysts currently used in industry can meet the conversion requirements of polymerization, their selectivity still needs to be improved.
[0004] In recent years, with the continuous development of catalytic materials research, researchers have prepared alkyne selective hydrogenation catalysts of different materials to achieve selective hydrogenation of unsaturated alkynes. Zhou et al. used g-C3N4 as a support and loaded Ni catalyst, achieving complete conversion of acetylene in the temperature range of 175-300℃ with a reaction selectivity of over 63% (doi.org / 10.1021 / acssuschemeng.1c07263).
[0005] Maligal-Ganesh et al. achieved efficient selective hydrogenation removal of acetylene by preparing a PtSn catalyst on the surface of a SiO2 support and then coating it with mesoporous silica. At 200 °C, the acetylene conversion was 93% and the ethylene selectivity was 81% (doi.org / 10.1002 / cctc.202000155).
[0006] Riley et al. prepared a Ni single-atom catalyst using CeO2 as a support, achieving a near 100% conversion of acetylene to ethylene. However, the reaction temperature was as high as 200℃ (doi.org / 10.1002 / cctc.201801976).
[0007] However, while these reactions can achieve efficient conversion of alkynes under specific conditions, they still require reaction temperatures exceeding 150°C to achieve complete removal of alkynes. This is still far from the conditions required for real industrial applications and cannot meet the actual needs of factories. Summary of the Invention
[0008] To address the problems in existing technologies, this invention proposes a method for the pre-hydrogenation reaction of acetylene. The catalyst of this invention, prepared by combining specific active components with a composite support, exhibits high catalytic activity. This catalyst can be directly used in the pre-hydrogenation reaction of acetylene, improving both the conversion rate and selectivity of the selective hydrogenation of acetylene to ethylene.
[0009] One objective of this invention is to provide a method for the pre-hydrogenation reaction of acetylene, comprising the following steps:
[0010] The feed gas containing acetylene and hydrogen undergo a hydrogenation reaction in the presence of a catalyst.
[0011] The catalyst comprises a composite support and an active component supported on the composite support;
[0012] The composite carrier includes carrier A and carrier B, wherein carrier A is graphene-coated nanodiamond.
[0013] The carrier B is at least one of inorganic oxides, diatomaceous earth, and molecular sieves;
[0014] The active component is palladium.
[0015] In this invention, carrier B uses irregularly shaped carriers such as spheres, sheets, toothed spheres, strips, clover leaves, or four-leaf clovers.
[0016] In the method for the pre-hydrogenation reaction of acetylene described in this invention, preferably,
[0017] In the raw material gas,
[0018] The mole fraction of acetylene is 0.1%–10.0%; and / or,
[0019] The mole fraction of hydrogen is 1–30%; and / or,
[0020] The temperature for hydrogenation reactions is 10–180 °C;
[0021] The space velocity of the hydrogenation reaction is 1000–20000 h⁻¹. -1 ;
[0022] Preferably,
[0023] The mole fraction of acetylene is 0.1%–6%; and / or,
[0024] The molar fraction of hydrogen is 5–25%; and / or,
[0025] The temperature for the hydrogenation reaction is 20–120°C; more preferably 50–120°C; even more preferably 60–120°C; and / or,
[0026] The space velocity of the hydrogenation reaction is 5000–12000 h⁻¹. -1 Further preferred is 6000–10000h -1 .
[0027] In the method for the pre-hydrogenation reaction of acetylene described in this invention, preferably,
[0028] Based on the weight of carrier A and carrier B as 100%, the proportion of carrier A is 5-40 wt%; preferably 15-35 wt%; and / or,
[0029] The specific surface area of the composite carrier is 1-400 m². 2 / g; preferably 280m 2 / g-400m 2 / g.
[0030] In the method for the pre-hydrogenation reaction of acetylene described in this invention, preferably,
[0031] The inorganic oxide is selected from at least one of Al2O3, SiO2, TiO2, and MgO.
[0032] In the method for the pre-hydrogenation reaction of acetylene described in this invention, preferably,
[0033] Based on the weight of the composite carrier as 100%,
[0034] The active component palladium is 0.01–0.2 wt% of the composite carrier, preferably 0.01–0.1 wt%; and / or,
[0035] In the catalyst, the active component palladium has a particle size range of 0.1–3 nm, preferably 0.2–1 nm.
[0036] In the method for the pre-hydrogenation reaction of acetylene described in this invention, preferably,
[0037] The preparation method of the graphene-coated nanodiamond includes the following steps:
[0038] The nanodiamonds prepared by detonation were calcined under a protective atmosphere to obtain the graphene-coated nanodiamonds.
[0039] In the method for pre-hydrogenation reaction of acetylene described in this invention, preferably, nanodiamonds are placed in a tubular furnace and calcined under a protective atmosphere to obtain the graphene-coated nanodiamonds.
[0040] In the catalyst with a composite support described in this invention, the nanodiamond obtained by detonation can be prepared using existing conventional methods or by purchasing existing materials. Preferably,
[0041] The graphene-coated nanodiamond has a core-shell structure with graphene as the shell and nanodiamond as the core; in the core-shell structure, the number of graphene shell layers is 1-3.
[0042] In the method for the pre-hydrogenation reaction of acetylene described in this invention, preferably,
[0043] The nanodiamond has a particle size of 10–200 nm; and / or,
[0044] The calcination temperature is 900–1500 °C; and / or,
[0045] The roasting time is 3 to 6 hours;
[0046] Preferably,
[0047] The calcination temperature is 900–1200°C; and / or,
[0048] The roasting time is 3 to 6 hours.
[0049] In the method for the pre-hydrogenation reaction of acetylene described in this invention, preferably,
[0050] The catalyst is prepared by:
[0051] The catalyst was prepared by loading palladium onto a composite support;
[0052] Preferably, the catalyst is prepared by loading a palladium-containing precursor compound solution onto the composite support via impregnation or deposition precipitation, followed by post-treatment.
[0053] In the method for the pre-hydrogenation reaction of acetylene described in this invention, preferably,
[0054] In the palladium-containing precursor compound solution, the palladium-containing precursor compound is selected from palladium salts; and / or,
[0055] The amount of palladium added to the palladium-containing precursor compound solution is 0.01–0.2 wt% of the weight of the composite support; preferably,
[0056] The palladium salt is selected from at least one of inorganic palladium salts and organic palladium salts; and / or,
[0057] The amount of palladium added to the palladium-containing precursor compound solution is 0.01 to 0.1 wt% of the weight of the composite carrier;
[0058] More preferably,
[0059] The inorganic palladium salt is selected from at least one of palladium chloride, palladium nitrate, and palladium sulfate; and / or,
[0060] The organic palladium salt is selected from at least one of palladium acetate and palladium acetylacetonate; and / or,
[0061] In the palladium-containing precursor compound solution, the concentration of palladium is 0.01-200 mg / mL.
[0062] In the method for the pre-hydrogenation reaction of acetylene described in this invention, preferably,
[0063] The solvent in the palladium-containing precursor compound solution is selected from at least one of inorganic solvents and organic solvents; and / or,
[0064] The post-processing includes washing and drying.
[0065] Preferably,
[0066] The inorganic solvent is selected from at least one of water, hydrochloric acid, and nitric acid; and / or,
[0067] The organic solvent is selected from at least one of acetic acid and ethanol; and / or,
[0068] The drying temperature in the post-treatment is 50–200°C; and / or,
[0069] The drying time in the post-treatment is 5 to 48 hours;
[0070] More preferably,
[0071] When the inorganic solvent is selected from an aqueous hydrochloric acid solution, the molar concentration of the aqueous hydrochloric acid solution is 0.001-0.1; and / or,
[0072] When the inorganic solvent is selected from an aqueous nitric acid solution, the molar concentration of the aqueous nitric acid solution is 0.001-0.1; and / or,
[0073] The drying temperature in the post-treatment is 80–120°C; and / or,
[0074] The drying time in the post-treatment is 5 to 24 hours.
[0075] In the method for the pre-hydrogenation reaction of acetylene described in this invention, preferably,
[0076] The composite carrier is prepared by mixing carrier A, carrier B and adhesive, and then molding to obtain the composite carrier.
[0077] Preferably, the adhesive is selected from at least one of carboxymethyl cellulose, polyvinyl alcohol, and starch; and / or,
[0078] The adhesive content is 1-30 wt%, based on the total weight of carrier A and carrier B as 100%.
[0079] In this invention, the composite carrier is formed using existing conventional molding processes, such as compression molding, extrusion molding, spray drying molding, oil molding, jet granulation molding, cooling granulation molding, and fibrous carrier molding. Molding conditions can be selected from commonly used molding parameters.
[0080] In the method for the pre-hydrogenation reaction of acetylene described in this invention, preferably,
[0081] The deposition and precipitation method includes the following steps: dispersing the composite support in water, adjusting the pH value to 9-10 to obtain a dispersion; then adjusting the pH value of the palladium-containing precursor compound solution to 6-7 and adding it dropwise to the dispersion, heating and stirring, and drying to obtain the catalyst;
[0082] More preferably, a sodium carbonate solution is used to adjust the pH value; the heating and stirring conditions are to keep the mixture at 80-100°C in an oil bath and stir for 1-2 hours.
[0083] In the method for the pre-hydrogenation reaction of acetylene described in this invention, preferably,
[0084] The impregnation method includes the following steps: mixing the vacuum-treated composite support with a palladium-containing precursor compound solution, impregnating and stirring, and drying to obtain the catalyst;
[0085] More preferably, the impregnation and stirring temperature is 35-45℃ for 3-5 hours.
[0086] In the preparation method of the present invention, drying can be carried out in an air atmosphere or under vacuum.
[0087] In the preparation method of this invention, the active component precursor can be loaded onto the support using the impregnation method employed in catalyst preparation, such as equal-volume impregnation or supersaturated impregnation. When using the supersaturated impregnation method, if the active component precursor in the impregnation solution cannot be completely adsorbed by the support, the volume of the impregnation solution and the concentration of the active component should be determined according to the adsorption ratio to ensure that the content of the active component loaded onto the support meets the predetermined requirements.
[0088] The selective hydrogenation catalyst described in this invention can be analyzed using X-ray photoelectron spectroscopy (XPS) to confirm the chemical valence state of the active component of the catalyst; the particle size and particle size distribution of the active component can be observed using transmission electron microscopy (TEM); and the distribution of the active component on the surface and cross-section of the support can be observed using scanning electron microscopy (SEM).
[0089] In the method for pre-hydrogenation of acetylene described in this invention, preferably, the pre-hydrogenation reaction step includes:
[0090] (A) The above catalyst is loaded into the reactor;
[0091] (B) The feed gas containing acetylene is introduced into the reactor to carry out the selective hydrogenation reaction of acetylene.
[0092] In this invention, the reactor is a conventional hydrogenation reactor in the art.
[0093] The endpoints and any values of the ranges disclosed in this invention are not limited to the precise ranges or values; these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein. In the following, various technical solutions can, in principle, be combined with each other to obtain new technical solutions, which should also be considered as specifically disclosed herein.
[0094] Compared with the prior art, the present invention has at least the following advantages:
[0095] The catalyst prepared by the present invention through a composite support has high catalytic activity. When the catalyst prepared by the present invention is used in the pre-hydrogenation reaction of acetylene, the conversion rate and selectivity of selective hydrogenation of acetylene to ethylene are improved.
[0096] The catalyst of this invention can be directly used in the pre-hydrogenation reaction of acetylene, and the catalyst of this invention still has good catalytic effect at low temperature, making it suitable for industrial production. Detailed Implementation
[0097] The present invention will now be described in detail with reference to specific embodiments. It should be noted that the following embodiments are only used to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the content of the present invention are still within the scope of protection of the present invention.
[0098] It should also be noted that the various specific technical features described in the following embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the various possible combinations will not be described separately in this invention.
[0099] Furthermore, various embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention. The resulting technical solutions are part of the original disclosure of this specification and also fall within the protection scope of the present invention.
[0100] Unless otherwise specified, the raw materials used in the examples and comparative examples are all disclosed in the prior art, such as those that can be directly purchased or prepared according to the preparation methods disclosed in the prior art.
[0101] Preparation Example 1
[0102] Preparation method of graphene-coated nanodiamonds:
[0103] Nanodiamonds prepared by detonation were calcined under nitrogen at a temperature of 1200°C for 5 hours to obtain graphene-coated nanodiamonds. The graphene-coated nanodiamonds prepared by the above method have a core-shell structure with graphene as the shell and nanodiamond as the core; in the core-shell structure, the number of graphene shell layers is 1-3.
[0104] Preparation Example 2
[0105] Preparation method of composite carrier:
[0106] The composite carrier was prepared by mixing carrier A (graphene-coated nanodiamond prepared in Preparation Example 1), carrier B, and binder starch, followed by cooling and granulation. The specific composition of the composite carrier is shown in Tables 1 and 3.
[0107] Example 1
[0108] Measure 200 mL of deionized water into a flask, add 0.1 M Na₂CO₃ solution to adjust the pH to 10, then weigh 4.5 g of the composite carrier and add it to the above solution. Preheat the solution in a 100°C oil bath. Weigh a certain amount of Pd. 2+A 0.4 mg / mL Pd(NO3)2 solution was added dropwise to the support after adjusting the pH to neutral with 0.1 M Na2CO3 solution. The mixture was stirred in an oil bath at 100 °C for 2 h. After the reaction, the mixture was cooled to room temperature, filtered, and washed with deionized water until the filtrate was neutral. The resulting catalyst was then dried in an oven at 60 °C for 12 h and labeled as catalyst A. The specific composition is shown in Table 2.
[0109] Examples 2-4
[0110] Following the method of Example 1, except that the carrier mixed with the graphene-coated nanodiamond carrier is different, the prepared catalysts are labeled as catalyst B, catalyst C, and catalyst D, respectively, and their specific compositions are shown in Table 2.
[0111] Table 1
[0112]
[0113] Table 2
[0114]
[0115]
[0116] Example 5
[0117] 10.2 g of the composite carrier was placed in a rotary evaporator and evacuated for 10 min. A certain amount of Pd was measured. 2+ A 0.4 mg / mL Pd(NO3)2 solution was diluted to 100 mL with deionized water. This solution was added dropwise to the support, and the mixture was impregnated and stirred at 40 °C for 5 h. After cooling to room temperature, 50 mL of C2H5OH was added to the solution, and the solvent was removed using a rotary evaporator. The resulting catalyst was dried in a 60 °C oven for 12 h and labeled as catalyst E. Its specific composition is shown in Table 4.
[0118] Examples 6-8
[0119] Following the method of Example 5, except that the carrier mixed with the graphene-coated nanodiamond carrier is different, the prepared catalysts are labeled as catalyst E, catalyst F, and catalyst G, respectively, and their specific compositions are shown in Table 4.
[0120] Table 3
[0121]
[0122]
[0123] Table 4
[0124]
[0125] In the preparation of the catalyst of the present invention, the content of the active component is calculated according to the fact that the active component is completely adsorbed on the support, and the corresponding palladium nitrate solution is added at a concentration of 0.4 mg / mL.
[0126] Comparative Example 1
[0127] A Pd-Ag / Al2O3 catalyst was prepared as a comparative example using the traditional impregnation method. 5 mL of a 10 mg Pd / mL palladium nitrate solution was diluted with water to 70 mL and then impregnated with 100 g of a catalyst with a specific area of 30 m² / mL. 2 The catalyst was prepared by placing a spherical Al2O3 support at 120°C and drying it for 8 hours. Then, it was immersed in an aqueous silver nitrate solution (0.047 g of silver nitrate was prepared into 60 mL of silver nitrate solution), dried at 120°C for 8 hours, and calcined at 600°C with air for 4 hours to obtain the Pd-Ag catalyst.
[0128] Comparative Example 2
[0129] The preparation method is basically the same as that of Example 1, except that in Comparative Example 2, the Al2O3 support in Example 1 is replaced with an equal mass of graphene-coated nanodiamond support, denoted as Catalyst I.
[0130] Comparative Example 3
[0131] The preparation method is basically the same as that of Example 1, except that in Comparative Example 2, the graphene-coated nanodiamond support in Example 1 is replaced with an equal mass of Al2O3 support, which is referred to as catalyst II.
[0132] Example 9
[0133] The prepared catalyst was subjected to a simulated microreactor experiment for the pre-hydrogenation reaction of acetylene under the following reaction conditions:
[0134] 2g of catalyst was packed into a stainless steel tube reactor with an inner diameter of 2mm. After purging with nitrogen, the feed gas simulating pre-ethane removal and pre-hydrogenation was introduced into the reactor. The composition (mole fraction) of the feed gas was: C2H2: 0.101%, C2H6: 12.06%, C2H4 equilibrium, H2: 23.60%, CO: 0.0812%, and the experimental space velocity was 15000 h⁻¹. -1 .
[0135] The catalytic performance of the above catalysts for the selective hydrogenation of acetylene before hydrogenation was evaluated. Catalyst AH in the examples was evaluated directly, catalysts in Comparative Examples 2-3 were evaluated directly, and catalyst in Comparative Example 1 was evaluated after hydrogen reduction. The conversion and selectivity of acetylene hydrogenation to ethylene for each catalytic reaction at 60°C are listed in Table 5. The calculation methods for the conversion and selectivity of acetylene hydrogenation to ethylene before hydrogenation are as follows:
[0136]
[0137]
[0138] Table 5. Simulation results of the pre-hydrogenation process (60℃)
[0139]
[0140]
[0141] By comparing Comparative Example 1 with Examples 1-4, it can be seen that the catalyst prepared by the composite support of the present invention has higher selectivity and conversion rate in hydrogenation reaction compared with the commonly used Pd-Ag catalyst. This result fully demonstrates that the catalyst prepared by the composite support of the present invention has better performance.
[0142] Comparing Comparative Example 2 with Example 1, it can be seen that the catalyst prepared by the composite support of the present invention exhibits higher selectivity and conversion rate in the hydrogenation reaction. Comparing Comparative Example 3 with Example 1, it can be seen that the catalyst prepared by the composite support of the present invention exhibits higher selectivity and conversion rate in the hydrogenation reaction. In summary, the above results fully demonstrate that support A and support B of the present invention have a direct synergistic effect, and the catalyst corresponding to the composite support prepared by them has better performance.
[0143] Examples 10-13
[0144] The reaction conditions are basically the same as those in Example 9, except that the reaction temperatures in Examples 10-13 are replaced with 40°C, 70°C, 100°C, and 120°C respectively. The specific results are shown in Table 6.
[0145] Table 6. Experimental Results for Evaluation of Pre-Hydrogenation Reaction
[0146]
[0147]
[0148] Based on the above data, it can be seen that the catalyst of the present invention does not require a high reaction temperature, and has excellent conversion rate and selectivity even at reaction temperatures below 100°C, meeting the actual reaction conditions of the plant.
[0149] The present invention has been described in detail above with reference to specific embodiments and exemplary examples; however, these descriptions should not be construed as limiting the present invention. Those skilled in the art will understand that various equivalent substitutions, modifications, or improvements can be made to the technical solutions and embodiments of the present invention without departing from the spirit and scope of the invention, and all such modifications and improvements fall within the scope of the present invention. The scope of protection of the present invention is defined by the appended claims.
Claims
1. A method for a pre-hydrogenation reaction of acetylene, characterized in that, Includes the following steps: The feed gas containing acetylene and hydrogen undergo a hydrogenation reaction in the presence of a catalyst. The catalyst comprises a composite support and an active component supported on the composite support; The composite carrier includes carrier A and carrier B, wherein carrier A is graphene-coated nanodiamond. The carrier B is at least one of inorganic oxides, diatomaceous earth, and molecular sieves; the inorganic oxide is selected from at least one of Al2O3, SiO2, TiO2, and MgO. The active component is palladium; based on the weight of the supports A and B as 100%, the proportion of support A is 5~40 wt%; in the catalyst, the particle size range of the active component palladium is 0.1~3 nm.
2. The method for pre-hydrogenation reaction of acetylene according to claim 1, characterized in that: In the raw material gas, The mole fraction of acetylene is 0.1% to 10.0%; and / or, The mole fraction of hydrogen is 1-30%; and / or, The temperature for hydrogenation reactions is 10~180℃; The space velocity of the hydrogenation reaction is 1000~20000 h⁻¹. -1 .
3. The method for pre-hydrogenation reaction of acetylene according to claim 2, characterized in that: The mole fraction of acetylene is 0.1% to 6%; and / or, The mole fraction of hydrogen is 5-25%; and / or, The temperature for hydrogenation reactions is 20–120 °C; and / or, The space velocity of the hydrogenation reaction is 5000 ~ 12000 h⁻¹ -1 .
4. The method for pre-hydrogenation reaction of acetylene according to claim 3, characterized in that: The temperature for hydrogenation is 50~120℃; and / or, The space velocity of the hydrogenation reaction is 6000~10000 h⁻¹. -1 .
5. The method for pre-hydrogenation reaction of acetylene according to claim 4, characterized in that: The temperature for hydrogenation reaction is 60~120℃.
6. The method for pre-hydrogenation reaction of acetylene according to claim 1, characterized in that: Based on the total weight of carrier A and carrier B being 100%, the proportion of carrier A is 15-35 wt%; and / or, The specific surface area of the composite carrier is 1-400 m². 2 / g.
7. The method for pre-hydrogenation reaction of acetylene according to claim 6, characterized in that: The specific surface area of the composite carrier is 280 m². 2 / g-400m 2 / g.
8. The method for pre-hydrogenation reaction of acetylene according to claim 1, characterized in that: Based on the weight of the composite carrier as 100%, The active component palladium is 0.01~0.2 wt% of the composite carrier; and / or, In the catalyst, the active component palladium has a particle size range of 0.2~1 nm.
9. The method for pre-hydrogenation reaction of acetylene according to claim 8, characterized in that: The active component palladium is 0.01~0.1 wt% of the composite carrier.
10. The method for pre-hydrogenation reaction of acetylene according to claim 1, characterized in that, The preparation method of the graphene-coated nanodiamond includes the following steps: The nanodiamonds prepared by detonation were calcined under a protective atmosphere to obtain the graphene-coated nanodiamonds.
11. The method for pre-hydrogenation reaction of acetylene according to claim 10, characterized in that: The graphene-coated nanodiamond has a core-shell structure with graphene as the shell and nanodiamond as the core; in the core-shell structure, the number of graphene shell layers is 1-3.
12. The method for pre-hydrogenation reaction of acetylene according to claim 10, characterized in that: The nanodiamond has a particle size of 10~200 nm; and / or, The calcination temperature is 900~1500℃; and / or, The roasting time is 3-6 hours.
13. The method for pre-hydrogenation reaction of acetylene according to claim 12, characterized in that: The calcination temperature is 900~1200℃; and / or, The roasting time is 3 to 6 hours.
14. The method for pre-hydrogenation reaction of acetylene according to any one of claims 1-13, characterized in that: The catalyst is prepared by: The catalyst was prepared by loading palladium onto a composite support.
15. The method for pre-hydrogenation reaction of acetylene according to claim 14, characterized in that: The catalyst is prepared by loading a palladium-containing precursor compound solution onto the composite support via impregnation or deposition precipitation, followed by post-treatment.
16. The method for pre-hydrogenation reaction of acetylene according to claim 15, characterized in that: In the palladium-containing precursor compound solution, the palladium-containing precursor compound is selected from palladium salts; and / or, The amount of palladium added to the palladium-containing precursor compound solution is 0.01~0.2 wt% of the weight of the composite carrier.
17. The method for pre-hydrogenation reaction of acetylene according to claim 16, characterized in that: The palladium salt is selected from at least one of inorganic palladium salts and organic palladium salts; and / or, The amount of palladium added to the palladium-containing precursor compound solution is 0.01~0.1 wt% of the weight of the composite carrier.
18. The method for pre-hydrogenation reaction of acetylene according to claim 17, characterized in that: The inorganic palladium salt is selected from at least one of palladium chloride, palladium nitrate, and palladium sulfate; and / or, The organic palladium salt is selected from at least one of palladium acetate and palladium acetylacetonate; and / or, In the palladium-containing precursor compound solution, the concentration of palladium is 0.01-200 mg / mL.
19. The method for pre-hydrogenation reaction of acetylene according to claim 15, characterized in that: The solvent in the palladium-containing precursor compound solution is selected from at least one of inorganic solvents and organic solvents; and / or, The post-processing includes washing and drying.
20. The method for pre-hydrogenation reaction of acetylene according to claim 19, characterized in that: The inorganic solvent is selected from at least one of water, hydrochloric acid, and nitric acid; and / or, The organic solvent is selected from at least one of acetic acid and ethanol; and / or, The drying temperature in the post-treatment is 50~200℃; and / or, The drying time in the post-treatment is 5 to 48 hours.
21. The method for pre-hydrogenation reaction of acetylene according to claim 20, characterized in that: The drying temperature in the post-treatment is 80~120℃; and / or, The drying time in the post-processing is 5 to 24 hours.
22. The method for pre-hydrogenation reaction of acetylene according to claim 14, characterized in that: The composite carrier is prepared by mixing carrier A, carrier B and adhesive, and then molding the mixture to obtain the composite carrier.
23. The method for pre-hydrogenation reaction of acetylene according to claim 22, characterized in that: The adhesive is selected from at least one of carboxymethyl cellulose, polyvinyl alcohol, and starch; and / or, The content of the adhesive is 1 to 30 wt%, based on the total weight of carrier A and carrier B as 100%.
Citation Information
Patent Citations
Acetylene selective hydrogenation catalyst and preparation method and application thereof
CN101862653A
Atomic-scale dispersed palladium-based nanometer diamond / graphene composite material catalyst, preparation method and applications thereof
CN109174085A