A branched fluoropolymer, its preparation method and use

Branched fluoropolymers were prepared by a branched copolymerization method under normal pressure, which solved the problems of high synthesis difficulty and poor controllability in traditional methods, achieved high monomer conversion rate and improved conductivity, and expanded the application range.

CN117946317BActive Publication Date: 2026-11-20FUDAN UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410072039.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-18
Publication Date
2026-11-20
Estimated Expiration
2044-01-18

AI Technical Summary

Technical Problem

Existing fluoropolymers are difficult to synthesize, with challenging structures and properties. Traditional methods offer poor control over branched structures and limited monomer conversion rates, making them unsuitable for a wider range of applications.

Method used

A branched fluoropolymer was prepared by using a branched copolymerization method under normal pressure conditions, through the polymerization of fluorinated monomers, comonomers and chain transfer monomers, to control the degree of branching and thermodynamic properties, and to introduce different functional groups.

Benefits of technology

The synthesis of fluoropolymers with controllable branching degree was achieved, with high monomer conversion rate. When applied to lithium-ion solid electrolytes, the conductivity was significantly improved, expanding the application range of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117946317B_ABST
    Figure CN117946317B_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of synthesis of fluorine-containing copolymer, and particularly relates to a branched fluorine-containing polymer and a preparation method thereof. The branched fluorine-containing polymer is successfully synthesized by polymerizing fluorine-containing monomers, comonomers and chain transfer monomers. By adjusting the molar ratio of the comonomers and the chain transfer monomers, the branching degree of the polymer can be flexibly regulated. The polymerization method has the advantages of simple operation, wide monomer application range, high monomer conversion rate and controllable branching degree. The application provides strong support for expanding the synthesis method of the fluorine-containing polymer and the application of the fluorine-containing polymer in different fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of novel fluoropolymer material development, specifically relating to a branched fluoropolymer, its preparation method, and its application in solid electrolytes for lithium-ion batteries. Background Technology

[0002] The topological structure of polymers has a significant impact on their physicochemical properties. Among them, branched polymers, as an important class of polymer materials, are characterized by less molecular chain entanglement and abundant terminal functional groups compared to linear polymers. This special topological structure endows polymers with unique properties, such as low viscosity, high solubility, and high reactivity, making them widely used in biomedicine, catalysis, materials modification, and other fields.

[0003] Fluoropolymers possess excellent comprehensive properties. For example, polyvinylidene fluoride (PVDF) and its copolymer derivatives combine the characteristics of fluoropolymers and general-purpose resins, and have been widely used in electronics, petrochemicals, and defense industries, becoming the preferred polymer materials. However, the synthesis of main-chain fluoropolymers such as PVDF is difficult, and their structure and properties are hard to tune, thus limiting their processing efficiency and application range. Controlling the branching structure of polymers has greatly enriched the types and properties of polymer materials. For example, the novel Kynar high melt strength (HMS) PVDF produced by Arkema in the United States has a long-chain branched structure that improves the polymer's rheological properties, and its mechanical properties are comparable to traditional linear PVDF resins, making it suitable for more processing technologies and application fields. Traditional free radical polymerization is the main method for preparing fluoropolymers. The reaction needs to be carried out under high temperature and high pressure, resulting in limited monomer conversion, difficulty in introducing functional groups, and difficulty in precisely controlling the polymer's topology. For example, the preparation of branched PVDF resins relies on chain transfer mechanisms under high temperature and high pressure conditions, and the controllability of the branching structure is poor. Meanwhile, existing reports on the controlled synthesis of branched fluoropolymers focus on the study of fluorinated acrylate monomers, while research on fluorinated olefin monomers is relatively limited. Summary of the Invention

[0004] To address existing problems, this invention proposes an improved synthesis strategy aimed at overcoming the limitations of traditional methods and providing strong support for the innovative development of fluoropolymer materials. The objective of this invention is to provide a branched fluoropolymer and its preparation method, capable of synthesizing a main-chain fluoropolymer with a well-defined degree of branching.

[0005] It should be noted that this method can synthesize branched copolymers of fluoroolefins (such as trifluorochloroethylene, hexafluoropropylene, tetrafluoroethylene, and perfluorovinyl ether) under normal pressure conditions, with controllable branching degree, high monomer conversion rate, and a wide range of applicable comonomers. By increasing the branching degree of polymers with similar molecular weights, their glass transition temperature and viscosity can be significantly reduced. Furthermore, branched fluoropolymers can be used in lithium-ion solid electrolytes, and polymer electrolytes with high branching degree exhibit significantly improved conductivity compared to those with low branching degree.

[0006] To achieve the above objectives, the present invention adopts the following technical solution:

[0007] The first technical objective of this invention is to provide a branched fluoropolymer having the structural formula shown in formula (1):

[0008]

[0009] Among them, R 1 The structure consists of a trifluoromethyl group, a chlorine atom, a fluorine atom, a perfluoroalkoxy group with a chain length of C1 to C8, and derivatives thereof; R 2 The structure is derived from alkoxy, ester, pyrrolidone, and the above groups; n is an integer between 1 and 8; x, y, and z are the degrees of polymerization corresponding to the repeating units.

[0010] The second technical objective of this invention is to provide a method for preparing the branched fluoropolymer as described above.

[0011] To achieve the above objectives, the present invention adopts the following technical solution:

[0012] A method for preparing the branched fluoropolymer as described above, wherein the preparation method comprises:

[0013] (a) Prepare a reaction solution and deoxygenate the reaction system to make the inside of the container a nitrogen-protected environment, wherein the reaction solution includes fluorinated monomers, comonomers, chain transfer monomers, solvents, and reaction aids;

[0014] (b) React under light or heating conditions for 6 to 24 hours; after the reaction is complete, the reaction solution is added dropwise to a poor solvent to precipitate three times, separated, and dried to obtain the branched fluoropolymer.

[0015] More preferably, the structure of the fluorinated monomer is shown in formulas (2) to (4):

[0016]

[0017] Among them, R 1 It is a perfluoroalkoxy group consisting of a trifluoromethyl group, a chlorine atom, a fluorine atom, and a chain length of C1 to C8, R.3 It is a derivative structure such as sulfonyl fluoride, where m is an integer of 1 or 2.

[0018] More preferably, the comonomer includes vinyl ether monomers and their derivatives, vinyl ester monomers and their derivatives, vinyl pyrrolidone monomers and their derivatives, and the structure of the comonomer is shown in formulas (5) to (7):

[0019]

[0020] In equation (5), R 4 It is an alkyl group having 1 to 12 carbon atoms or an ethylene glycol group having 1 to 18 repeating units or a derivative structure of the above groups; in formula (6), R 5 It is a derivative structure of an alkyl, aryl or above group having 1 to 12 carbon atoms; in formula (7), p is an integer between 1 and 3.

[0021] More preferably, the structure of the chain transfer monomer is as shown in formula (8):

[0022]

[0023] Among them, R 6 It is an alkoxy group with 1 to 12 carbon atoms, a trifluoroalkoxy group with 1 to 11 carbon atoms, or an alkyl mercapto group with 1 to 12 carbon atoms; R 7 It consists of hydrogen atoms, alkyl groups with 1 to 12 carbon atoms, or cyano groups; R 8 It consists of hydrogen atoms and alkyl or cyano groups with 1 to 12 carbon atoms.

[0024] More preferably, the organic solvent is one or a combination of several selected from N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, dimethyl carbonate, diethyl carbonate, ethyl acetate, dichloromethane, methanol, ethanol, trifluoroethanol, hexafluoroisopropanol, trichlorobenzene, n-hexane, n-pentane, dioxane, tetrahydrofuran, toluene, anisole, dichloromethane, acetone, and acetonitrile; the reaction aid includes one or a combination of several selected from photocatalysts, alkylamines, photoinitiators, and thermal initiators.

[0025] In some embodiments, the photocatalyst comprises one or more combinations of small organic molecule compounds with a skeleton of perylene, pyrene, porphyrin, thiophene, phenothiazine, phenoxazine, or isophthalonitrile, or metal-organic complexes with a core of copper, ruthenium, iridium, or zinc; the alkylamine comprises one or more combinations of triethylamine, tetramethylethylenediamine, pentamethyldiethylenetriamine, and triethanolamine; the thermal initiator comprises one or more combinations of azo compounds such as azobisisobutyronitrile and peroxide compounds such as benzoyl peroxide; and the photoinitiator comprises one or more combinations of 2,4,6-(trimethylbenzoyl)diphenylphosphine oxide, benzoin, and benzophenone.

[0026] More preferably, the monomer molar ratio in step (a) is:

[0027] The molar ratio of fluorinated monomer to chain transfer monomer is (1-100):1; the molar ratio of comonomer to chain transfer monomer is (0-100):100.

[0028] The reaction conditions described in step (b) are: the emission wavelength of the light source is 200-780 nm, and the reaction temperature is room temperature to 200 °C.

[0029] In step (b), the volume ratio of the reaction solution to the unsuitable solvent is 1:(5-20).

[0030] The second technical objective of this invention is to provide an application of the branched fluoropolymer described above in a metal battery or a metal-ion battery.

[0031] Specifically, the branched fluoropolymer is used in the solid electrolyte of lithium-ion batteries.

[0032] Compared with existing technologies, the present invention has the following superior effects:

[0033] The branched fluoropolymer of this invention is prepared by polymerizing fluorinated monomers, comonomers, and chain transfer monomers. By flexibly adjusting the molar ratio of comonomers to chain transfer monomers, the degree of branching and thermodynamic properties of the polymer were successfully controlled. Furthermore, by changing the type of comonomer, different functional groups were successfully introduced. The proposed polymer exhibits controllable branching and structural properties, the preparation method is simple, the monomers have a wide range of applicability, and the monomer conversion rate is high, providing a new approach for the development of novel fluorinated materials. Simultaneously, when this branched polymer is applied to the solid electrolyte of lithium-ion batteries, the conductivity can be significantly improved by controlling the degree of branching. This research provides strong support for innovation in the field of fluoropolymers and the development of new materials. Attached Figure Description

[0034] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.

[0035] Figure 1 This is a schematic diagram of the synthetic route for the small molecule in Example 1.

[0036] Figure 2 This is a schematic diagram of the synthesis route of the polymer in Example 2.

[0037] Figure 3 The GPC-RI spectra of the polymers in Examples 4 and 5 are shown.

[0038] Figure 4 The polymer in Example 5 1 H NMR spectrum.

[0039] Figure 5 The polymer in Example 5 19 F NMR spectrum.

[0040] Figure 6 The graphs show the thermogravimetric analysis of the polymers in Examples 4 and 5.

[0041] Figure 7 Differential scanning calorimetry (DSC) spectra of the polymers in Examples 4 and 5 are shown.

[0042] Figure 8 The time-scan rheograms of the polymers in Examples 4 and 5 at 20°C are shown.

[0043] Figure 9 The conductivity diagrams are for the polymer electrolytes in Examples 4 and 5. Detailed Implementation

[0044] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0045] The term "embodiment" used herein, as an example, is not necessarily to be construed as superior to or better than other embodiments. Performance testing in the embodiments of this application, unless otherwise specified, employs conventional testing methods in the art. It should be understood that the terminology used in this application is merely for describing particular implementations and is not intended to limit the scope of this disclosure.

[0046] Unless otherwise stated, the technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; other experimental methods and technical means not specifically mentioned herein refer to experimental methods and technical means commonly used by one of ordinary skill in the art.

[0047] To better illustrate the content of this application, numerous specific details are provided in the following detailed embodiments. Those skilled in the art should understand that this application can be implemented even without certain specific details. In the embodiments, some methods, means, instruments, and devices well-known to those skilled in the art are not described in detail in order to highlight the main points of this application.

[0048] Without conflict, the technical features disclosed in the embodiments of this application can be combined arbitrarily, and the resulting technical solution belongs to the content disclosed in the embodiments of this application.

[0049] To better understand the present invention, the following embodiments are provided for further detailed description of the invention, but they should not be construed as limiting the invention. Any non-essential improvements and adjustments made by those skilled in the art based on the above description are also considered to fall within the protection scope of the present invention.

[0050] Example 1

[0051] 0.62 g (10.0 mmol) of ethanethiol, 0.67 g (12.0 mmol) of potassium hydroxide, and 20 mL of acetone were added to a glass flask equipped with a stir bar, and the mixture was stirred for 2 hours. Then, 0.91 g (12.0 mmol) of carbon disulfide was slowly added dropwise to the flask at room temperature, and the mixture was stirred for 2 hours. Subsequently, 1.53 g (10.0 mmol) of 2-bromopropionic acid was added to the flask at room temperature, and the mixture was stirred overnight. After the reaction was complete, the reaction solution was extracted, dried, and concentrated for preliminary purification. The concentrate was used directly in the next reaction step. The concentrate (10.0 mmol), 2.47 g (12.0 mmol) of N,N'-dicyclohexylcarbodiimide, 60 mg (0.5 mmol) of 4-dimethylaminopyridine, and 25 mL of dichloromethane were added to a glass bottle equipped with a stir bar. 1.32 g (15.0 mmol) of ethylene glycol ether was slowly added dropwise under ice bath conditions. The mixture was stirred and reacted overnight. After the reaction was complete, the reaction solution was concentrated and purified by column chromatography to obtain 2.54 g of 2-(ethoxy)ethyl 2-(ethyl trithiocarbonate)propionate, with a yield of 86%.

[0052] Example 2

[0053] 4.3 g (10.0 mmol) of 2-perfluoropropoxyperfluoropropyltrifluorovinyl ether, 0.5 g (5.0 mmol) of vinyl n-butyl ether, 28.0 mg (0.1 mmol) of 2-(ethoxy)ethyl 2-(ethyl trithiocarbonate)propionate, and 8.2 mg (5.0 × 10⁻⁶) of azobisisobutyronitrile (AIBN) were added. -2 5 mmol of toluene was added to a glass bottle equipped with a stir bar. The air atmosphere in the reaction system was replaced with nitrogen, the system was sealed, and the reaction was stirred at 70°C for 24 hours. The conversion rate of the monomer was measured to be 99% by gas chromatography. The reaction solution was added dropwise to methanol to precipitate the solid, which was then separated and dried to obtain a pale yellow solid.

[0054] The polymer was analyzed using gel permeation chromatography-multi-angle laser light scattering and 400MHz Fourier transform nuclear magnetic resonance spectroscopy. The results are as follows:

[0055] M n,MALLS =1.1×10 5 g / mol and molecular weight distribution M w / M n =2.65, branching degree DB=0.027.

[0056] Example 3

[0057] Vinyl n-butyl ether 0.5 g (5.0 mmol), 2-(ethoxy)ethyl 2-(ethyl trithiocarbonate)propionate 56.0 mg (0.2 mmol), 2,4,6-(trimethylbenzoyl)diphenylphosphine oxide 0.9 mg (2.5 × 10⁻⁶) -3 5 mL of toluene (25 mmol) was added to a glass bottle equipped with a stir bar, and finally 2.9 g (25 mmol) of trifluorochloroethylene was introduced. The air atmosphere in the reaction system was replaced with nitrogen, sealed, and stirred for 24 hours under the illumination of a 20W white LED lamp (wavelength 380 nm~780 nm). The conversion rate of the monomer was measured to be 99% by gas chromatography. The reaction solution was added dropwise to methanol to precipitate the solid, which was then separated and dried to obtain a pale yellow solid.

[0058] The polymer was analyzed using gel permeation chromatography-multi-angle laser light scattering and 400MHz Fourier transform nuclear magnetic resonance spectroscopy. The results are as follows:

[0059] M n,MALLS =7.5×10 4 g / mol and molecular weight distribution M w / M n =2.08, branching degree DB=0.041.

[0060] Example 4

[0061] The following ingredients were added: 2.66 g (10.0 mmol) of perfluoropropyl vinyl ether, 0.73 g (5.0 mmol) of (2-(2-methoxyethoxy)ethoxy)ethylene, 0.14 g (0.5 mmol) of 2-(ethoxy)ethyl 2-(ethyl trithiocarbonate)propionate, and 0.9 mg (2.5 × 10⁻⁶) of 2,4,6-(trimethylbenzoyl)diphenylphosphine oxide. -3 5 mmol) of toluene was added to a glass bottle equipped with a stir bar. The air atmosphere in the reaction system was replaced with nitrogen, the system was sealed, and the reaction was stirred for 24 hours under the illumination of a 20W white LED lamp (wavelength 380nm~780nm). The conversion rate of the monomer was measured to be 99% by gas chromatography. The reaction solution was added dropwise to methanol to precipitate the solid, which was then separated and dried to obtain a pale yellow solid.

[0062] The polymer was analyzed using gel permeation chromatography-multi-angle laser light scattering and 400MHz Fourier transform nuclear magnetic resonance spectroscopy. The results are as follows:

[0063] M n,MALLS =4.7×10 4 g / mol and molecular weight distribution M w / M n =1.92, branching degree DB=0.156, 5% thermal decomposition temperature T5%d =329℃, glass transition temperature T g = -9.9℃, viscosity η* = 2.6 × 10 6 mPa s.

[0064] Example 5

[0065] The following ingredients were added: 2.66 g (10.0 mmol) of perfluoropropyl vinyl ether, 0.73 g (5.0 mmol) of (2-(2-methoxyethoxy)ethoxy)ethylene, 0.28 g (1.0 mmol) of 2-(ethoxy)ethyl 2-(ethyl trithiocarbonate)propionate, and 1.6 mg (2.5 × 10⁻⁶) of tris(2-phenylpyridine)iridium. -3 5 mmol) of toluene was added to a glass bottle equipped with a stir bar. The air atmosphere in the reaction system was replaced with nitrogen, the system was sealed, and the reaction was stirred for 24 hours under the illumination of a 20W white LED lamp (wavelength 380nm~780nm). The conversion rate of the monomer was measured to be 99% by gas chromatography. The reaction solution was added dropwise to methanol to precipitate the solid, which was then separated and dried to obtain a pale yellow solid.

[0066] The polymer was analyzed using gel permeation chromatography-multi-angle laser light scattering and 400MHz Fourier transform nuclear magnetic resonance spectroscopy. The results are as follows:

[0067] M n,MALLS =3.8×10 4 g / mol and molecular weight distribution M w / M n =1.80, branching degree DB=0.243, 5% thermal decomposition temperature T 5%d =311℃, glass transition temperature T g = -21.1℃, viscosity η* = 1.7 × 10 6 mPa s.

[0068] Example 6

[0069] Vinyl n-butyl ether 0.5 g (5.0 mmol), 2-(ethoxy)ethyl 2-(ethyl trithiocarbonate)propionate 0.7 g (2.5 mmol), tris(2-phenylpyridine)iridium 1.6 mg (2.5 × 10⁻⁶) -3 5 mL of toluene (25 mmol) was added to a glass bottle equipped with a stir bar, and finally 3.75 g (25 mmol) of hexafluoropropylene was introduced. The air atmosphere in the reaction system was replaced with nitrogen, sealed, and stirred for 24 hours under irradiation with a 20 W ultraviolet lamp (wavelength 395 nm to 400 nm). The conversion rate of the monomer was measured to be 99% by gas chromatography. The reaction solution was added dropwise to methanol to precipitate the solid, which was then separated and dried to obtain a pale yellow solid.

[0070] The polymer was analyzed using gel permeation chromatography-multi-angle laser light scattering and 400MHz Fourier transform nuclear magnetic resonance spectroscopy. The results are as follows:

[0071] M n,MALLS =2.7×10 4 g / mol and molecular weight distribution M w / M n =1.73, branching degree DB=0.383.

[0072] Example 7

[0073] 1.16 g (10.0 mmol) of perfluoromethyl vinyl ether, 0.5 g (5.0 mmol) of vinyl n-butyl ether, 1.4 g (5.0 mmol) of 2-(ethoxy)ethyl 2-(ethyl trithiocarbonate)propionate, and 1.6 mg (2.5 × 10⁻⁶) of tris(2-phenylpyridine)iridium were added. -3 5 mmol) of toluene was added to a glass bottle equipped with a stir bar. The air atmosphere in the reaction system was replaced with nitrogen, the system was sealed, and the reaction was stirred for 24 hours under the illumination of a 20W white LED lamp (wavelength 380nm~780nm). The conversion rate of the monomer was measured to be 99% by gas chromatography. The reaction solution was added dropwise to methanol to precipitate the solid, which was then separated and dried to obtain a pale yellow solid.

[0074] The polymer was analyzed using gel permeation chromatography-multi-angle laser light scattering and 400MHz Fourier transform nuclear magnetic resonance spectroscopy. The results are as follows:

[0075] M n,MALLS =1.4×10 4 g / mol and molecular weight distribution M w / M n =1.66, branching degree DB=0.443.

[0076] Example 8

[0077] Vinyl n-butyl ether 0.5 g (5.0 mmol), 2-(ethoxy)ethyl 2-(ethyl trithiocarbonate)propionate 0.28 g (1.0 mmol), tris(2-phenylpyridine)iridium 1.6 mg (2.5 × 10⁻⁶) -3 5 mL of toluene (25 mmol) was added to a glass bottle equipped with a stir bar, and finally 2.5 g (25 mmol) of tetrafluoroethylene was introduced. The air atmosphere in the reaction system was replaced with nitrogen, sealed, and stirred for 24 hours under the illumination of a 20W white LED lamp (wavelength 380 nm–780 nm). The conversion rate of the monomer was measured to be 99% by gas chromatography. The reaction solution was added dropwise to methanol to precipitate the solid, which was then separated and dried to obtain a pale yellow solid.

[0078] The polymer was analyzed using gel permeation chromatography-multi-angle laser light scattering and 400MHz Fourier transform nuclear magnetic resonance spectroscopy. The results are as follows:

[0079] M n,MALLS =3.1×10 4 g / mol and molecular weight distribution M w / M n =1.79, branching degree DB=0.231.

[0080] Example 9

[0081] The following ingredients were added: 2.66 g (10 mmol) of perfluoropropyl vinyl ether, 0.44 g (5.0 mmol) of ethylene glycol vinyl ether, 0.14 g (0.5 mmol) of 2-(ethoxy)ethyl 2-(ethyl trithiocarbonate)propionate, and 1.6 mg (2.5 × 10⁻⁶) of tris(2-phenylpyridine)iridium. -3 5 mmol) of toluene was added to a glass bottle equipped with a stir bar. The air atmosphere in the reaction system was replaced with nitrogen, the system was sealed, and the reaction was stirred for 24 hours under the illumination of a 20W white LED lamp (wavelength 380nm~780nm). The conversion rate of the monomer was measured to be 99% by gas chromatography. The reaction solution was added dropwise to dichloromethane to precipitate the solid, which was then separated and dried to obtain a pale yellow solid.

[0082] The polymer was analyzed using gel permeation chromatography-multi-angle laser light scattering and 400MHz Fourier transform nuclear magnetic resonance spectroscopy. The results are as follows:

[0083] M n,MALLS =3.9×10 4 g / mol and molecular weight distribution M w / M n =1.93, branching degree DB=0.133.

[0084] Example 10

[0085] 2.44 g (10 mmol) of 4,5-difluoro-2,2-bis(trifluoromethyl)-1,3-dioxanepentene, 0.5 g (5.0 mmol) of vinyl n-butyl ether, 0.14 g (0.5 mmol) of 2-(ethoxy)ethyl 2-(ethyl trithiocarbonate)propionate, and 1.6 mg (2.5 × 10⁻⁶) of tris(2-phenylpyridine)iridium were added. -35 mmol) of toluene was added to a glass bottle equipped with a stir bar. The air atmosphere in the reaction system was replaced with nitrogen, the system was sealed, and the reaction was stirred for 24 hours under the illumination of a 20W white LED lamp (wavelength 380nm~780nm). The conversion rate of the monomer was measured to be 99% by gas chromatography. The reaction solution was added dropwise to methanol to precipitate the solid, which was then separated and dried to obtain a pale yellow solid.

[0086] The polymer was analyzed using gel permeation chromatography-multi-angle laser light scattering and 400MHz Fourier transform nuclear magnetic resonance spectroscopy. The results are as follows:

[0087] M n,MALLS =4.2×10 4 g / mol and molecular weight distribution M w / M n =2.01, branching degree DB=0.139.

[0088] Example 11

[0089] Fluoropolymers with different degrees of branching obtained in Examples 4 and 5 were dissolved in acetonitrile with lithium bis(trifluoromethanesulfonylimide) (1 wt% of the polymer) and stirred for 2 hours. The solvent was concentrated and dried in a vacuum oven at 70°C for 48 hours. The mixture was then used as a solid electrolyte and filled into a CR 2032 symmetric cell. The ionic conductivity was tested at 30°C to 90°C using a CHI electrochemical workstation.

[0090] At 90°C, the electrical conductivity of the branched polymers corresponding to Examples 4 and 5 is 1.7 × 10⁻⁶. -4 S cm -1 and 3.1×10 -4 S cm -1 By increasing the degree of branching of the polymer, the electrical conductivity was increased by 1.8 times.

[0091] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a branched fluoropolymer, characterized in that, The specific steps of the method are as follows: (a) Prepare the reaction solution and deoxygenate the reaction system to make the inside of the container a nitrogen-protected environment, wherein the reaction solution includes fluorinated monomers, comonomers, chain transfer monomers, solvents, and reaction aids; (b) React under light or heating conditions for 6 to 24 hours; after the reaction is complete, the reaction solution is added dropwise to a poor solvent to precipitate, and after separation and drying, the branched fluoropolymer is obtained. The structural formulas of the fluorine-containing monomers are shown in formulas (2) to (4): ; Among them, R 1 Selected from perfluoroalkoxy groups with chain lengths of trifluoromethyl, chlorine, fluorine, and C1 to C8, R 3 Selected from sulfonyl fluoride and trifluoromethyl, where m is an integer of 1 or 2; The comonomers include vinyl ether monomers and their derivatives, vinyl ester monomers and their derivatives, and vinyl pyrrolidone monomers and their derivatives. The structural formulas of the comonomers are shown in formulas (5) to (7): ; In equation (5), R 4 It is an alkyl group having 1 to 12 carbon atoms, an ethylene glycol group having 1 to 18 repeating units, or a derivative structure of the above groups; in formula (6), R 5 It is a derived structure of an alkyl, aryl or above group having 1 to 12 carbon atoms; in formula (7), p is an integer between 1 and 3; The chain transfer monomer structure is shown in equation (8): ; Among them, R 6 It consists of alkoxy groups with 1 to 12 carbon atoms, trifluoroalkoxy groups with 1 to 12 carbon atoms, and alkyl mercapto groups with 1 to 12 carbon atoms; R 7 It consists of hydrogen atoms and alkyl or cyano groups having 1 to 12 carbon atoms; R 8 It consists of hydrogen atoms and alkyl or cyano groups with 1 to 12 carbon atoms; n is an integer between 1 and 8.

2. The method for preparing branched fluoropolymers according to claim 1, characterized in that, The molar ratio of the fluorinated monomer to the chain transfer monomer is (1 ~ 100):1, and the molar ratio of the comonomer to the chain transfer monomer is (0 ~ 100):

1.

3. The method for preparing branched fluoropolymers according to claim 1, characterized in that, The solvent is N,N -Dimethylformamide, N,N - One or more combinations of dimethylacetamide, dimethyl sulfoxide, dimethyl carbonate, diethyl carbonate, ethyl acetate, dichloromethane, methanol, ethanol, trifluoroethanol, hexafluoroisopropanol, trichlorobenzene, n-hexane, n-pentane, dioxane, tetrahydrofuran, toluene, anisole, dichloromethane, acetone, and acetonitrile; the reaction aid is one or more combinations of photocatalyst, alkylamine, photoinitiator, and thermal initiator.

4. The method for preparing branched fluoropolymers according to claim 1, characterized in that, The illumination conditions described herein involve an emission wavelength of 200-780 nm from the light source; the heating conditions involve a temperature ranging from room temperature to 200 nm. o C; The volume ratio of the reaction solution to the unsuitable solvent is 1:(5~20).

5. A branched fluoropolymer prepared by the method of claim 1.

6. The application of a branched fluoropolymer prepared by the method of claim 1 or the branched fluoropolymer of claim 5 in a metal battery or a metal-ion battery.

7. The application according to claim 6, characterized in that, Application of the branched fluoropolymer in solid electrolytes for lithium-ion batteries.

Citation Information

Patent Citations

  • Synthesis method of fluoropolymer rich in boric acid ester and hydroxyl