A memory alloy composite solid lubricating film material, a preparation method and application thereof

By using a composite material of shape memory alloys and layered transition metal dichalcogenides, a solid lubricating film with low friction coefficient, high friction life and intelligent responsiveness in a vacuum environment was prepared, solving the problem of poor friction performance of traditional films in a vacuum environment.

CN117946780BActive Publication Date: 2026-11-20LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410112700.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-26
Publication Date
2026-11-20
Estimated Expiration
2044-01-26

AI Technical Summary

Technical Problem

Existing technologies struggle to provide highly stable and long-life intelligent lubricating films in a vacuum environment, and traditional solid lubricating films exhibit poor frictional performance under varying loads and rotational speeds.

Method used

A composite material of shape memory alloy and layered transition metal dichalcogenides is used to form a shape memory alloy composite solid lubricating film on the substrate surface by physical vapor deposition, thereby optimizing its tribological properties and intelligent responsiveness.

Benefits of technology

It achieves a low coefficient of friction and a long friction life in a vacuum environment, possesses intelligent responsiveness, adapts to changes in load and speed, and exhibits excellent lubrication performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117946780B_ABST
    Figure CN117946780B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of solid lubrication, and particularly relates to a memory alloy composite solid lubrication film material, a preparation method and application thereof. The present application provides a memory alloy composite solid lubrication film material, and preparation raw materials include shape memory alloy and layered transition metal dichalcogenide; the mass ratio of the shape memory alloy and the layered transition metal dichalcogenide is (1-30):100. The memory alloy composite solid lubrication film material has better tribological performance (in a vacuum environment) and also has intelligent responsiveness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solid lubrication technology, and in particular to a shape memory alloy composite solid lubrication film material, its preparation method, and its application. Background Technology

[0002] With the rapid development of space exploration and the application of various new precision aerospace vehicles, the requirements for the mechanical lubrication performance of core components are becoming increasingly stringent. Therefore, designing and fabricating highly stable, long-life, and intelligent lubrication films is imperative. Shape memory alloys (SMAs) are materials composed of two or more metallic elements that exhibit shape memory effects, capable of undergoing reversible phase transformations under stress or heating conditions. SMAs also possess superelasticity, allowing them to recover their shape under external forces without fatigue deformation. Solid lubricating films (SLFs) are an effective way to reduce wear between mating components in moving mechanisms and are crucial for ensuring the stable operation of space moving parts. Utilizing the superelasticity of shape memory alloys to enhance the yield and springback capabilities of solid lubricating films, thereby improving their lubrication performance and enabling intelligent load response, is an effective method for preparing intelligent solid lubricating film materials. Summary of the Invention

[0003] The purpose of this invention is to provide a shape memory alloy composite solid lubricating film material, its preparation method, and its application. The shape memory alloy composite solid lubricating film material possesses high tribological properties (in a vacuum environment) and also exhibits intelligent responsiveness.

[0004] To achieve the above-mentioned objectives, the present invention provides the following technical solution:

[0005] This invention provides a shape memory alloy composite solid lubricating film material, the raw materials for which include shape memory alloy and layered transition metal dichalcogenides;

[0006] The mass ratio of the shape memory alloy to the layered transition metal dichalcogenide is (1-30):100.

[0007] Preferably, the shape memory alloy is Au-Cd, Ag-Cd, Cu-Zn, Cu-Zn-Al, Cu-Zn-Sn, Cu-Zn-Si, Cu-Sn, Cu-Zn-Ga, In-Ti, Au-Cu-Zn, NiAl, Fe-Pt, Ti-Ni, Ti-Ni-Pd, Ti-Nb, U-Nb, or Fe-Mn-Si.

[0008] Preferably, the chemical composition of the layered transition metal dichalcogenide is: MX2, where M is a group IV to VI transition metal and X is a chalcogenide element.

[0009] Preferably, M is W and / or Mo;

[0010] X is S and / or Se.

[0011] Preferably, the shape memory alloy and the layered transition metal disulfide compound have a structure of one or more of polycrystalline, microcrystalline, amorphous, quasicrystalline, and nanocrystalline.

[0012] This invention also provides a method for preparing the shape memory alloy composite solid lubricating film material described in the above technical solution, comprising the following steps:

[0013] The shape memory alloy composite solid lubricating film material is obtained by simultaneously sputtering a shape memory alloy target and a layered transition metal dichalcogenide target on the substrate surface using physical vapor deposition.

[0014] Preferably, the physical vapor deposition method is magnetron sputtering, radio frequency sputtering, DC sputtering, vacuum evaporation, arc plasma deposition, or ion deposition.

[0015] Preferably, the physical vapor deposition has a vapor deposition power of 10–600 W, a chamber pressure of 0.1–20 Pa, a bias voltage of 0–-500 V, and a time of 5–60 min.

[0016] The thickness of the shape memory alloy composite solid lubricating film material is 0.3–5.0 μm.

[0017] Preferably, the composite method of the shape memory alloy composite solid lubricating film material is doping composite or multilayer composite.

[0018] The present invention also provides the application of the shape memory alloy composite solid lubrication film material described in the above technical solution or the shape memory alloy composite solid lubrication film material prepared by the preparation method described in the above technical solution in the field of solid lubrication.

[0019] This invention provides a shape memory alloy composite solid lubricating film material, prepared from shape memory alloys and layered transition metal dichalcogenides; the mass ratio of the shape memory alloy to the layered transition metal dichalcogenides is (1-30):100. By doping the shape memory alloy with transition metal dichalcogenides, this invention reduces the surface roughness of the film, increases its elastic recovery and anti-adhesion capabilities, improves the tribological properties of the composite solid lubricating film in a vacuum environment, and also endows the film with a certain degree of intelligence. According to the embodiments, the shape memory alloy composite solid lubricating film material of this invention has a coefficient of friction of less than 0.05 and a lubrication life of more than 5.0 × 10⁻⁶ in a vacuum environment. 5 In the initial stage of lubrication, the coefficient of friction of the film is less than 0.01, and it increases with the increase of load. This material has certain application prospects in the field of space lubrication. Attached Figure Description

[0020] Figure 1 The XRD patterns are of the shape memory alloy composite solid lubricating film materials described in Examples 1-4 and the pure WS2 film described in Comparative Example 1.

[0021] Figure 2 The Raman spectra of the shape memory alloy composite solid lubricating film materials described in Examples 1-4 and the pure WS2 film described in Comparative Example 1 are shown.

[0022] Figure 3 The XRD patterns are of the shape memory alloy composite solid lubricating film material described in Example 3, the pure TiNb film described in Comparative Example 2, and the pure WS2 film described in Comparative Example 1.

[0023] Figure 4 SEM images of the shape memory alloy composite solid lubricating film materials described in Examples 1-4 and the pure WS2 film described in Comparative Example 1;

[0024] Figure 5 The friction curves of the shape memory alloy composite solid lubricating film materials described in Examples 1-4 and the pure WS2 film described in Comparative Example 1 are shown in the friction curves 20 minutes before the friction test.

[0025] Figure 6 The friction life curves of the shape memory alloy composite solid lubricating film materials described in Examples 1-4 and the pure WS2 film described in Comparative Example 1 are shown.

[0026] Figure 7 The wear rates of the shape memory alloy composite solid lubricating film materials described in Examples 1-4 and the pure WS2 film described in Comparative Example 1 are shown.

[0027] Figure 8The friction curves of the shape memory alloy composite solid lubricating film material described in Example 3 within 5 minutes at rotational speeds of 200 rpm, 400 rpm, 600 rpm, 800 rpm, 1000 rpm, 1200 rpm, and 1400 rpm.

[0028] Figure 9 The friction curves of the shape memory alloy composite solid lubricating film material described in Example 3 over 20 minutes under loads of 1N, 3N, 5N, and 7N, respectively.

[0029] Figure 10 The image shows the room temperature friction life curves of the shape memory alloy composite solid lubricating film material described in Example 3 under loads of 1N, 3N, 5N, and 7N.

[0030] Figure 11 The surface roughness of the shape memory alloy composite solid lubricating film material described in Example 3 and the pure WS2 film described in Comparative Example 1;

[0031] Figure 12 The DMT modulus of the shape memory alloy composite solid lubricating film material described in Example 3 and the pure WS2 film described in Comparative Example 1;

[0032] Figure 13 The adhesion between the shape memory alloy composite solid lubricating film material described in Example 3 and the pure WS2 film described in Comparative Example 1;

[0033] Figure 14 The Raman spectra of the surface of the paired spheres after friction tests on the shape memory alloy composite solid lubricating film material described in Example 3 and the pure WS2 film described in Comparative Example 1.

[0034] Figure 15 The TEM of the shape memory alloy multilayer composite solid lubricating film material described in Example 5. Detailed Implementation

[0035] This invention provides a shape memory alloy composite solid lubricating film material, the raw materials for which include shape memory alloy and layered transition metal dichalcogenides;

[0036] The mass ratio of the shape memory alloy to the layered transition metal dichalcogenide is (1-30):100.

[0037] In this invention, unless otherwise specified, all raw materials used in the preparation are commercially available products well known to those skilled in the art.

[0038] In this invention, the shape memory alloy is preferably Au-Cd, Ag-Cd, Cu-Zn, Cu-Zn-Al, Cu-Zn-Sn, Cu-Zn-Si, Cu-Sn, Cu-Zn-Ga, In-Ti, Au-Cu-Zn, NiAl, Fe-Pt, Ti-Ni, Ti-Ni-Pd, Ti-Nb, U-Nb, or Fe-Mn-Si.

[0039] In this invention, the preferred chemical composition of the layered transition metal dichalcogenide is MX2, wherein M is preferably a group IV to VI transition metal, more preferably W and / or Mo; X is preferably a chalcogenide element, more preferably S and / or Se. The chemical composition of the layered transition metal dichalcogenide is further preferably one or more of WS2, MoS2, and WSe2. When the layered transition metal dichalcogenide is two or more of the above-mentioned specific selections, this invention does not impose any special limitation on the proportions of the above-mentioned specific substances; they can be mixed in any proportion.

[0040] In this invention, the mass ratio of the shape memory alloy to the layered transition metal dichalcogenide is (1-30):100, preferably (5-25):100, and more preferably (10-20):100.

[0041] In this invention, the shape memory alloy and the layered transition metal disulfide compound are preferably one or more of the following: polycrystalline, microcrystalline, amorphous, quasicrystalline, and nanocrystalline.

[0042] This invention also provides a method for preparing the shape memory alloy composite solid lubricating film material described in the above technical solution, comprising the following steps:

[0043] The shape memory alloy composite solid lubricating film material is obtained by simultaneously sputtering a shape memory alloy target and a layered transition metal dichalcogenide target on the substrate surface using physical vapor deposition.

[0044] In this invention, the substrate is preferably 9Cr18 steel, titanium alloy, single-crystal silicon, quartz glass, or conductive glass. Before physical vapor deposition, the substrate is preferably pretreated. This pretreatment preferably includes: ultrasonically cleaning the substrate sequentially with water, petroleum ether, acetone, and anhydrous ethanol for 5–30 min; drying it; and fixing it on a rotatable substrate stage in the sputtering chamber. A TiNb target with a purity of 99.999% and a WS2 target with a purity of 99.9% are respectively fixed on the two RF guns of the magnetron sputtering instrument. The target front baffle is closed, and the gas pressure in the sputtering chamber is evacuated to 0.1–10 × 10⁻⁶. -3Below Pa, 99.999% pure argon gas is introduced at a flow rate of 30 sccm, and the sputtering chamber pressure is maintained at 8.0 Pa. The substrate surface is then cleaned with Ar ions for 10–30 min. The sputtering chamber pressure is then evacuated to 0.1–10 × 10⁻⁶ Pa. -3 Below Pa, 99.999% pure argon gas is introduced at a flow rate of 30 sccm, the sputtering chamber pressure is maintained at 8.0 Pa, and the bias voltage is -500 V. The substrate surface is cleaned for 10–50 min.

[0045] In this invention, the physical vapor deposition method is preferably magnetron sputtering, radio frequency sputtering, DC sputtering, vacuum evaporation, arc plasma deposition, or ion deposition, and more preferably radio frequency sputtering, magnetron sputtering, or DC sputtering.

[0046] In this invention, the thickness of the shape memory alloy composite solid lubricating film material is preferably 0.3–5.0 μm, more preferably 0.8–1.5 μm. In this invention, the thickness and composition of the shape memory alloy composite solid lubricating film material are preferably adjusted by the power of vapor deposition, chamber pressure, bias voltage, and deposition time.

[0047] In this invention, the physical vapor deposition power is preferably 10-600W, more preferably 100-500W, and most preferably 200-400W; the chamber pressure is preferably 0.1-20Pa, more preferably 5-15Pa, and most preferably 8-12Pa; the bias voltage is preferably 0--500V, more preferably -100--400V, and most preferably 200-300V; and the time is preferably 5-60min, more preferably 10-50min, and most preferably 20-30min.

[0048] In this invention, the composite method of the shape memory alloy composite solid lubricating film material is preferably doping composite or multilayer composite.

[0049] When the composite solid lubricating film material of the shape memory alloy is composited by doping, the composited method is preferably achieved by co-sputtering with ≥2 targets, and the doping concentration is preferably adjusted by changing the sputtering power of the shape memory alloy target. In this invention, the total number of co-sputtering targets is preferably 2 to 10, more preferably 3 to 8; the number of layered transition metal dichalcogenide targets is preferably greater than or equal to the number of shape memory alloy targets, that is, the number of layered transition metal dichalcogenide targets accounts for ≥1 / 2 of the total number of co-sputtering targets. In this invention, the number of layered transition metal dichalcogenide targets is preferably 2 to 4, more preferably 1 to 3. In this invention, the vapor deposition power of the shape memory alloy target is preferably 10 to 400 W, more preferably 50 to 200 W.

[0050] When the shape memory alloy composite solid lubricating film material is composited in a multilayer manner, the doping composite method is preferably adjusted by the substrate rotation speed, the target sputtering switching frequency, and the sputtering power of the shape memory alloy target. In this invention, the substrate rotation speed is preferably 1-20 rpm, more preferably 3-8 rpm; the target sputtering switching frequency is preferably controlled by a target front baffle, and the number of opening and closing times during the entire sputtering process is preferably 0-20 times, more preferably 2-5 times. In this invention, the sputtering power of the shape memory alloy target is preferably 10-400 W, more preferably 50-200 W.

[0051] This invention also provides the application of the shape memory alloy composite solid lubricating film material described in the above-described technical solutions, or the shape memory alloy composite solid lubricating film material prepared by the preparation method described in the above-described technical solutions, in the field of solid lubrication. This invention does not impose any special limitations on the methods for these applications; methods well-known to those skilled in the art can be used.

[0052] The following detailed description, in conjunction with embodiments, illustrates the shape memory alloy composite solid lubricating film material, its preparation method, and its applications provided by the present invention. However, these descriptions should not be construed as limiting the scope of protection of the present invention.

[0053] Example 1

[0054] The substrate (material 9Cr18 steel or silicon wafer) was ultrasonically cleaned sequentially with water, petroleum ether, acetone, and anhydrous ethanol for 20 minutes each. After drying, it was fixed on the rotatable substrate stage in the sputtering chamber. A TiNb target with a purity of 99.999% and a WS2 target with a purity of 99.9% were respectively fixed on the two RF guns of the magnetron sputtering instrument, and the target front baffle was closed. The gas pressure in the sputtering chamber was evacuated to 3 × 10⁻⁶. -3 Argon gas with a purity of 99.999% was introduced at a flow rate of 30 sccm. The sputtering chamber pressure was 8.0 Pa, and the bias voltage was -500 V. The substrate surface was cleaned with Ar ions for 30 min. After cleaning, the sputtering chamber pressure was reduced to 5 Pa, the bias voltage was reduced to -60 V, the baffle was opened, the sample turntable was started at a speed of 2 rpm, the power supplies of the two targets were turned on, the sputtering power of the WS2 target was adjusted to 300 W, the sputtering power of the TiNb target was adjusted to 50 W, and the sputtering time was 10 min to obtain a shape memory alloy doped composite solid lubricating film.

[0055] Example 2

[0056] Referring to Example 1, the difference is that the sputtering power of the TiNb target is 100W, the sputtering power of the WS2 target is 300W, and the sputtering time is 10min, to obtain a shape memory alloy doped composite solid lubricant film.

[0057] Example 3

[0058] Referring to Example 1, the difference is that the sputtering power of the TiNb target is 150W, the sputtering power of the WS2 target is 300W, and the sputtering time is 10min, to obtain a shape memory alloy doped composite solid lubricant film.

[0059] Example 4

[0060] Referring to Example 1, the difference is that the sputtering power of the TiNb target is 200W, the sputtering power of the WS2 target is 300W, and the sputtering time is 10min, to obtain a shape memory alloy doped composite solid lubricant film.

[0061] Example 5

[0062] Referring to Example 1, the difference is that the sputtering power of the TiNb target is 150W, the sputtering power of the WS2 target is 300W, the sputtering time is 20min, the turntable speed is 5rpm, and the target front baffle is opened and closed 4 times during this period to obtain a shape memory alloy multilayer composite solid lubricating film.

[0063] Comparative Example 1

[0064] Referring to Example 1, the difference is that the sputtering power of the TiNb target is 0W, the sputtering power of the WS2 target is 300W, and the sputtering time is 20min, resulting in a pure WS2 thin film.

[0065] Comparative Example 2

[0066] Referring to Example 1, the difference is that the sputtering power of the TiNb target is 200W, the sputtering power of the WS2 target is 0W, and the sputtering time is 20min, resulting in a pure TiNb thin film.

[0067] Test case

[0068] The tribological properties and intelligent responsiveness of the shape memory alloy composite solid lubricating film materials described in Examples 1-4 and the pure WS2 film described in Comparative Example 1 under vacuum conditions were evaluated using a vacuum ball-disc friction tester: the paired friction pair consisted of 9Cr18 steel balls with a diameter of 8 mm.

[0069] Test conditions for vacuum tribological properties: normal load 5N, rotation radius 5mm, rotation speed 1000rpm, background vacuum of the friction test chamber better than 7.0×10⁻⁶. -3 Pa, the friction coefficient is set to be greater than 0.15 as lubrication failure, and the test temperature is room temperature;

[0070] Experimental conditions for intelligent responsiveness: normal load 1-7 N, rotation radius 5 mm, rotation speed 200-1400 rpm.

[0071] Figure 1 The XRD patterns are those of the shape memory alloy composite solid lubricating film materials described in Examples 1-4 and the pure WS2 film described in Comparative Example 5. Figure 1 It can be seen that as the sputtering power of TiNb target increases, the crystallinity of the composite film decreases and the XRD shifts to a smaller angle, indicating that the incorporation of TiNb alloy causes the unit cell of WS2 to increase in size and deform, proving that TiNb alloy can effectively enter the unit cell of WS2 film to form TiNb-WS2 composite film.

[0072] Figure 2 The Raman spectra of the shape memory alloy composite solid lubricating film materials described in Examples 1-4 and the pure WS2 film described in Comparative Example 5 are obtained from... Figure 2 It can be seen that as the sputtering power of TiNb target increases, the crystallinity of WS2 in the composite film decreases, and the WO3 phase in the film basically disappears, indicating that TiNb doping is beneficial to improving the oxidation resistance of the film.

[0073] Figure 3 The XRD patterns are those of the shape memory alloy composite solid lubricant film material described in Example 3, the pure TiNb film described in Comparative Example 2, and the pure WS2 film described in Comparative Example 1. Figure 3 It can be seen that weak diffraction peak signals of TiNb and WS2 can still be observed in the memory alloy composite solid lubricating film material, indicating that TiNb and WS2 crystal structures still exist in the composite film. These crystalline components are beneficial to maintaining the independence of their own performance.

[0074] Figure 4 The images show SEM images of the shape memory alloy composite solid lubricating film materials described in Examples 1-4 and the pure WS2 film described in Comparative Example 1 (where 0W corresponds to Comparative Example 1, 50W to Example 1, 100W to Example 2, 150W to Example 3, and 200W to Example 4). Figure 4 As can be seen from the surface morphology, the addition of TiNb alloy reduces the size of the lamellar crystals on the film surface and makes the surface more tortuous; the cross-sectional morphology shows that the addition of TiNb alloy gradually increases the thickness of the underlying dense layer, while the corresponding columnar layer becomes thinner, and the overall density of the film increases.

[0075] Figure 5 The friction curves of the shape memory alloy composite solid lubricating film materials described in Examples 1-4 and the pure WS2 film described in Comparative Example 1 are obtained from the friction curves of the film materials before the friction test, 20 minutes prior to the test. Figure 5 It can be seen that the shape memory alloy composite solid lubricating film material described in Examples 1 to 4 is inferior to the pure WS2 film described in Comparative Example 1, and the coefficient of friction of the composite film is less than 0.01 when the sputtering power of the TiNb target is 150W.

[0076] Figure 6The friction life curves of the shape memory alloy composite solid lubricating film materials described in Examples 1-4 and the pure WS2 film described in Comparative Example 1 are obtained from... Figure 6 It can be seen that the friction life of the shape memory alloy composite solid lubricating film materials described in Examples 1-4 is generally higher than that of the pure WS2 film, and the friction life of the composite film is the highest when the TiNb target sputtering power is 150W, exceeding 6.0×10. 5 r;

[0077] Figure 7 The wear rate of the shape memory alloy composite solid lubricating film material described in Examples 1-4 and the pure WS2 film described in Comparative Example 1 is determined by... Figure 7 It can be seen that the shape memory alloy composite solid lubricating film material described in Example 3 has the lowest wear rate, which is only 2.27 × 10⁻⁶. -8 mm 3 ·N -1 ·m -1 The wear rate is only one-tenth of that of the pure WS2 film described in Comparative Example 1. However, when the sputtering power is increased to 200W, the wear rate of the film increases sharply, which is caused by the excessive metal content in the film.

[0078] Figure 8 The friction curves of the shape memory alloy composite solid lubricating film material described in Example 3 over 5 minutes at rotational speeds of 200 rpm, 400 rpm, 600 rpm, 800 rpm, 1000 rpm, 1200 rpm, and 1400 rpm are shown below. Figure 8 It can be seen that as the rotational speed increases, the friction coefficient first increases and then decreases. Among them, the friction curve is the most stable and the friction coefficient is the lowest at 600 rpm, which is 0.008. This indicates that the shape memory alloy composite solid lubricating film material has a certain adaptability to rotational speed.

[0079] Figure 9 The friction curves of the shape memory alloy composite solid lubricating film material described in Example 3 over 20 minutes under loads of 1N, 3N, 5N, and 7N are shown below. Figure 9 It can be seen that as the load increases, the friction coefficient gradually increases, reaching a minimum of 0.004, indicating that the shape memory alloy composite solid lubricating film material has a certain intelligent response to the load, and the friction coefficient of the shape memory alloy composite solid lubricating film material under different loads is less than 0.01, exhibiting super lubrication performance.

[0080] Figure 10 The figures for the room temperature friction life curves of the shape memory alloy composite solid lubricating film material described in Example 3 are shown below, under loads of 1N, 3N, 5N, and 7N. Figure 10It can be seen that, regardless of the load, the friction life of the shape memory alloy composite solid lubricating film material can exceed 5.0 × 10⁻⁶. 5 r has good tribological properties;

[0081] The surface roughness of the shape memory alloy composite solid lubricating film material described in Example 3 and the pure WS2 film described in Comparative Example 1 were characterized using atomic force microscopy. Figure 11 The surface roughness of the shape memory alloy composite solid lubricating film material described in Example 3 and the pure WS2 film described in Comparative Example 1 is determined by... Figure 11 It can be seen that the surface roughness Ra of the pure WS2 film in Comparative Example 1 is 22.4 nm, while the surface roughness Ra of the shape memory alloy composite solid lubricating film material in Example 3 is only 10.0 nm. The reduction in film roughness is beneficial to reducing frictional resistance.

[0082] Figure 12 The DMT modulus of the shape memory alloy composite solid lubricating film material described in Example 3 and the pure WS2 film described in Comparative Example 1 is determined by... Figure 12 It can be seen that the average elastic modulus of the pure WS2 film surface is 0.55 GPa, while the average elastic modulus of the shape memory alloy composite solid lubricating film material described in Example 3 is 1.37 GPa. This indicates that the doping of TiNb shape memory alloy helps to increase the elasticity of the film, and that the lubricating film recovers elastically after being subjected to external pressure, thereby maintaining the complete composite film structure, which is beneficial for reducing the friction coefficient and extending the friction life.

[0083] Figure 13 The adhesion between the shape memory alloy composite solid lubricating film material described in Example 3 and the pure WS2 film described in Comparative Example 1 is determined by... Figure 13 It can be seen that the maximum adhesion of the pure WS2 film surface can reach 102nN, while the maximum adhesion of the shape memory alloy composite solid lubricating film material described in Example 3 is only 19nN, indicating that the shape memory alloy composite solid lubricating film material described in this invention is also a potential anti-adhesion material.

[0084] Figure 14 The Raman spectra of the surface of the paired spheres after friction tests were obtained from the shape memory alloy composite solid lubricating film material described in Example 3 and the pure WS2 film described in Comparative Example 1. Figure 14 It can be seen that the Raman spectrum signal intensity of the dual sphere surface after friction with the shape memory alloy composite solid lubricating film material described in Example 3 is higher, indicating that a more regular and better crystallinity WS2 transfer film is formed. This shows that the performance improvement of the lubricating film is not only related to the special film material structure, but also to the ability to form the transfer film.

[0085] Figure 15The TEM image of the shape memory alloy multilayer composite solid lubricating film material described in Example 5 is obtained from... Figure 15 It can be seen that by controlling the opening and closing frequency of the sample turntable and baffle, a multilayer composite solid film can be obtained, with a thickness of about 20 nm between each layer.

[0086] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A shape memory alloy composite solid lubricating film material, characterized in that, The raw materials for preparation include shape memory alloys and layered transition metal dichalcogenides; The mass ratio of the shape memory alloy to the layered transition metal dichalcogenide is (1~30):100; The shape memory alloy is Ti-Nb; The chemical composition of the layered transition metal dichalcogenide is: MX2, where M is a group IV to VI transition metal and X is a chalcogenide element.

2. The shape memory alloy composite solid lubricating film material as described in claim 1, characterized in that, The M is W and / or Mo; X is S and / or Se.

3. The shape memory alloy composite solid lubricating film material as described in claim 1 or 2, characterized in that, The shape memory alloy and the layered transition metal dichalcogenide have structures that are one or more of polycrystalline, microcrystalline, amorphous, quasicrystalline, and nanocrystalline.

4. The method for preparing the shape memory alloy composite solid lubricating film material according to any one of claims 1 to 3, characterized in that, Includes the following steps: The shape memory alloy composite solid lubricating film material is obtained by simultaneously sputtering a shape memory alloy target and a layered transition metal dichalcogenide target on the substrate surface using physical vapor deposition.

5. The preparation method according to claim 4, characterized in that, The physical vapor deposition method is magnetron sputtering, radio frequency sputtering, DC sputtering, vacuum evaporation, arc plasma deposition, or ion deposition.

6. The preparation method according to claim 4 or 5, characterized in that, The physical vapor deposition process has a vapor deposition power of 10~600W, a chamber pressure of 0.1~20Pa, a bias voltage of 0~-500V, and a time of 5~60min. The thickness of the shape memory alloy composite solid lubricating film material is 0.3~5.0μm.

7. The preparation method according to claim 6, characterized in that, The composite method of the shape memory alloy composite solid lubricating film material is doping composite or multilayer composite.

8. The application of the shape memory alloy composite solid lubricating film material according to any one of claims 1 to 3 or the shape memory alloy composite solid lubricating film material prepared by the preparation method according to any one of claims 4 to 7 in the field of solid lubrication.

Citation Information

Patent Citations

  • Intelligent driving M50-based self-lubricating material and preparation method therefor

    CN111349813A

  • Composite lubricating film as well as preparation method and application thereof

    CN115058688A