A TiO2@PANI core-shell hollow cubic nanoparticle electrorheological fluid and its preparation method
By coating the surface of titanium dioxide nanoparticles with polyaniline to form a TiO₂@PANI core-shell structure, the problem of insufficient conductivity of titanium dioxide electrorheological materials is solved, and the high efficiency of rheological properties and stability of electrorheological fluids are achieved, making them suitable for practical applications.
Patent Information
- Application Number
- CN202311340845.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-17
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-10-17
AI Technical Summary
Existing titanium dioxide electrorheological materials have insufficient conductivity, which limits their performance in electrorheological fluids, and traditional preparation methods pose safety risks and instability.
A low-temperature two-phase method was used to coat the surface of titanium dioxide nanoparticles with highly conductive polyaniline to form hollow cubic nanoparticles with a TiO₂@PANI core-shell structure. Electrorheological fluids were then prepared by in-situ polymerization and combined with dimethyl silicone oil to form a stable dispersed phase.
It improves the conductivity and polarization response of electrorheological fluids, enhances rheological properties, and is safe and non-toxic in preparation. The process is simple, the material has good stability, and it is suitable for practical research and development and production.
Smart Images

Figure CN117946796B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to an electrorheological fluid material and its preparation method, specifically to a TiO2@PANI core-shell hollow cubic nanoparticle electrorheological fluid and its preparation method. Background Technology
[0002] Electrorheological materials, as a novel type of intelligent material that responds rapidly to electric fields, have attracted widespread attention due to their enormous application prospects in electrical control devices. Electrorheological fluids, also known as ER fluids, typically consist of an insulating carrier fluid and polarized particles. When no electric field is applied, the polarized particles are randomly dispersed and exhibit liquid-like properties. When an electric field is applied, the liquid phase rapidly transforms into a solid-like structure, forming chain-like or columnar structures along the direction of the electric field, while its viscosity, yield stress, and other properties change. This process is reversible when the electric field disappears. This change in properties is called the electrorheological effect. Electrorheological fluids are particularly sensitive to electrical signals and respond rapidly, thus having broad development prospects in many fields, such as hydraulic transmission and automotive braking. Titanium dioxide used in this invention is an excellent material for electrorheological research, possessing many advantages suitable for electrorheology, including a high dielectric constant, convenient and quick preparation, and stable properties. Furthermore, composite materials are materials with special properties that can be obtained from individual nanoparticles. Therefore, given the insufficient conductivity of titanium dioxide, this invention enhances conductivity and polarization response by coating its surface with highly conductive polyaniline to form a TiO2@PANI core-shell electrorheological material, thereby giving it better performance.
[0003] The purpose of this invention is to provide a TiO2@PANI core-shell hollow cubic nanoparticle electrorheological fluid, in which the dispersed phase is cubic hollow titanium dioxide (TiO2) nanoparticles coated with polyaniline (PANI), and the continuous phase is dimethyl silicone oil. Scanning electron microscopy (SEM) and transmission electron microscopy (TEM) images reveal cubic hollow titanium dioxide with a porous surface and anisotropic shape, all of which enhance interfacial polarization, which is beneficial for electrorheological effects. Electrorheological fluids prepared from titanium dioxide have many advantages, including high rheological efficiency and simple preparation; however, their poor conductivity is one of the reasons limiting their performance. Polyaniline, on the other hand, has strong conductivity, and combining the two can enhance conductivity. Therefore, by coating the nanoparticles with highly conductive polyaniline to form a core-shell structure, the rheological properties of the electrorheological fluid are improved, resulting in a faster response. The prepared electrorheological fluid has a low density, excellent anti-settling properties, and is more stable. The entire preparation process is safe and risk-free, non-toxic and harmless. The three-step process is clear and easy to understand, and simple to operate. It is also adjustable, and different reagent ratios will result in different rheological properties.
[0004] The present invention also aims to provide a core-shell cubic hollow titanium dioxide nanoparticle prepared by low-temperature biphase coating synthesis of TiO2@PANI based on the preparation of hollow titanium dioxide, obtaining hollow cubic titanium dioxide nanoparticles through secondary hydrothermal treatment, and then uniformly coating the surface of the nanoparticles with polyaniline by in-situ polymerization at low temperature. The preparation process is as follows: first, cubic solid titanium fluoride is prepared by a first hydrothermal reaction, then a second hydrothermal reaction is performed to etch hollow cubic titanium dioxide, and then polyaniline is uniformly coated on the nanoparticles by in-situ polymerization under low temperature and continuous stirring, thereby preparing polyaniline-coated cubic hollow titanium dioxide core-shell nanoparticles. These nanoparticles, with a hollow cubic titanium oxide inner layer uniformly coated with polyaniline, exhibit a very distinct core-shell structure morphology. The entire preparation process is simple, the raw materials are inexpensive and readily available, and the electrorheological fluid prepared exhibits excellent performance, combining stability, anti-settling properties, and conductivity within a suitable range. Furthermore, the unique hollow and porous nanostructure corresponds to the surface effect, small size effect, and other characteristics unique to nanomaterials, providing a new research method for further study of electrorheological materials and facilitating in-depth research into the practical development and application of electrorheological materials.
[0005] The objective of this invention can be achieved through the following technical solutions:
[0006] The electrorheological fluid prepared in this invention has a dispersed phase of polyaniline-coated titanium dioxide core-shell hollow cubic nanoparticles and a continuous phase of dimethyl silicone oil.
[0007] The preparation steps of TiO2@PANI electrorheological fluid are as follows:
[0008] (1) Add 1.6 mL of hydrofluoric acid to 10 mL of acetic acid, stir continuously until uniform, then add 5 mL of TBT, continue stirring until uniform, and then put it into a reaction vessel. Heat to 200℃ for the first hydrothermal reaction for 12 hours. After the reaction is complete, wait for the temperature to drop to room temperature, then centrifuge and wash the product, and put it in an oven to dry overnight at 75℃.
[0009] (2) Dissolve the 0.5g solid sample obtained in the first step in 20mL of ultrapure water and stir continuously until the solution is mixed evenly. Then put it into the reaction vessel and heat it to 120℃ for the second hydrothermal reaction. The heating time is 3h. After the reaction is completed, wait for the temperature to drop to room temperature and then perform centrifugation and washing. Place it in an oven and dry it overnight at 75℃.
[0010] (3) Dissolve the solid sample obtained from the above reaction in 100 mL of ethanol and stir until homogeneous. While stirring, add 0.1 g CTAB, 6 mL aniline, and 0.2 mL acetic acid in sequence, stir until homogeneous, and place in an ice-water bath to continue stirring for two hours. This is recorded as sample number one. Then add 1 g ammonium persulfate to 20 mL of water and stir until homogeneous. This is recorded as sample number two. After stirring sample number one for two hours, slowly add solution number two to it while stirring continuously. Continue stirring for 1 hour, and then immediately centrifuge the sample. Wash twice with water and three times with ethanol, ensuring that the last wash is with ethanol. After washing, place in an oven at 75°C and dry overnight to obtain TiO2@PANI particles.
[0011] (4) The sample was mixed with dimethyl silicone oil at a weight ratio of 10% to prepare an electrorheological fluid.
[0012] Compared with the prior art, the present invention has the following significant technical advantages:
[0013] 1. The preparation method of this invention uses in-situ polymerization to obtain titanium dioxide, and then uses a low-temperature two-phase method to coat it to obtain core-shell structured nanoparticles. The whole process is relatively stable and the morphology of the particles is regular and uniform.
[0014] 2. The electrorheological fluid prepared by combining it with silicone oil exhibits excellent rheological properties, low density, simple processing flow, safe reaction, and is non-toxic and harmless. It fully combines the advantages of both materials, making it an improved comprehensive electrorheological material. The raw materials are inexpensive and readily available, the preparation ratio is adjustable, and the material is non-toxic and harmless, making it suitable for practical research and development and production. Attached Figure Description
[0015] Figure 1 Scanning electron microscope image of TiO2 obtained by secondary hydrothermal treatment
[0016] Figure 2 Transmission electron microscopy image of TiO2 obtained by secondary hydrothermal treatment
[0017] Figure 3 XRD pattern of TiO2 obtained by secondary hydrothermal treatment
[0018] Figure 4 Scanning electron microscope image of TiO2@PANI obtained using 4 mL aniline.
[0019] Figure 5 Transmission electron microscopy image of TiO2@PANI obtained using 4 mL aniline.
[0020] Figure 6 The relationship between shear stress and shear rate of TiO2@PANI nanoparticle electrorheological fluid obtained using 4 mL of aniline under different electric field strengths.
[0021] Figure 7The relationship between shear stress and shear rate of TiO2@PANI nanoparticle electrorheological fluid obtained using 2 mL of aniline under different electric field strengths.
[0022] Figure 8 The relationship between shear stress and shear rate of TiO2@PANI nanoparticle electrorheological fluid obtained using 5 mL of aniline under different electric field strengths.
[0023] Figure 9 Scanning electron microscope image of TiO2@PANI obtained using 6 mL aniline.
[0024] Figure 10 Transmission electron microscopy image of TiO2@PANI obtained using 6 mL aniline.
[0025] Figure 11 XRD pattern of TiO2@PANI obtained using 6 mL aniline
[0026] Figure 12 The relationship between shear stress and shear rate of TiO2@PANI nanoparticle electrorheological fluid obtained using 6 mL of aniline under different electric field strengths. Detailed Implementation
[0027] Example 1 (Preparation of TiO2@PANI nanoparticles using 4 mL aniline)
[0028] Add 1.6 mL of hydrofluoric acid to 10 mL of acetic acid, stir continuously until homogeneous, then add 5 mL of TBT, continue stirring until homogeneous, and transfer to a reaction vessel. Heat to 200 °C for the first hydrothermal reaction for 12 hours. After the reaction is complete, allow the temperature to drop to room temperature, then centrifuge and wash, and dry in an oven at 75 °C overnight. Dissolve 0.5 g of the solid sample obtained in the first step in 20 mL of ultrapure water, stir continuously until the solution is homogeneous, then transfer to a reaction vessel and heat to 120 °C for the second hydrothermal reaction for 3 hours. After the reaction is complete, allow the temperature to drop to room temperature, then centrifuge and wash, and dry in an oven at 75 °C overnight to obtain hollow cubic titanium dioxide. Figure 1 The image shows a scanning electron microscope (SEM) image of the prepared sample. The SEM image shows cubic titanium dioxide nanoparticles with unique morphology and particle sizes ranging from several hundred nanometers. Figure 2 The image shows a transmission electron microscope (TEM) image of the prepared sample. The TEM image reveals hollow, cubic-shaped particles, indicating a hollow structure. The XRD pattern is shown below. Figure 3As shown, the sample conforms to the XRD standard PDF card for titanium dioxide. The solid sample obtained from the above reaction was dissolved in 100 mL of ethanol and stirred until homogeneous. While stirring, 0.1 g of CTAB, 6 mL of aniline, and 0.2 mL of acetic acid were added sequentially. After stirring until homogeneous, the sample was placed in an ice-water bath and stirred for another two hours, designated as sample number one. Then, 1 g of ammonium persulfate was added to 20 mL of water and stirred until homogeneous, designated as sample number two. After stirring sample number one for two hours, solution number two was slowly added to it while continuously stirring, and stirring was continued for 1 hour. The sample was then immediately centrifuged, washing twice with water and three times with ethanol, ensuring the final wash was with ethanol. After washing, the sample was dried overnight in an oven at 75°C to obtain TiO2@PANI particles. Figure 4 The image shows a scanning electron microscope (SEM) image of TiO2@PANI. The SEM image shows that polyaniline particles are coated on the surface of cubic titanium dioxide, and the coating effect is relatively uniform. Figure 5 The image shows a transmission electron microscope (TEM) image of TiO2@PANI. The TEM image reveals that the interior is hollow, indicating a hollow structure. The darker color of the cubic surface also confirms the presence of a coating layer, proving that the sample has a cubic hollow core-shell structure.
[0029] At room temperature, 0.15 g of TiO2@PANI sample was added to 1.5 mL of silicone oil and ground evenly in a mortar to obtain the required electrorheological fluid (weight ratio 10%). The electrorheological properties of the sample were then tested. Figure 6 The graph shows the relationship between shear stress and shear rate of the obtained electrorheological fluid under different electric field intensities. It can be seen from the graph that the shear stress increases significantly after the application of an electric field. According to the electrorheological efficiency formula e = (η... E The calculation of -η0) / η0 yields the result at 3kV, 0.1s -1 The current-rate efficiency is 277.8, with a large variation range, indicating good current-rate performance.
[0030] Example 2 (Preparation of TiO2@PANI nanoparticles from 2 mL aniline)
[0031] Add 1.6 mL of hydrofluoric acid to 10 mL of acetic acid, stir continuously until homogeneous, then add 5 mL of TBT, continue stirring until homogeneous, and then transfer to a reaction vessel. Heat to 200°C for the first hydrothermal reaction for 12 hours. After the reaction is complete, allow the temperature to drop to room temperature, then centrifuge and wash, and place in an oven to dry overnight at 75°C. Dissolve 0.5 g of the solid sample obtained in the first step in 20 mL of ultrapure water, stir continuously until the solution is homogeneous, then transfer to a reaction vessel and heat to 120°C for the second hydrothermal reaction for 3 hours. After the reaction is complete, allow the temperature to drop to room temperature, then centrifuge and wash, and place in an oven to dry overnight at 75°C. The resulting titanium dioxide template is consistent with that obtained in Example 1, both being hollow cubic in shape. The solid sample obtained from the above reaction was dissolved in 80 mL of water and stirred until homogeneous. While stirring, 0.1 g of CTAB, 2 mL of aniline, and 0.05 mL of acetic acid were added sequentially. The mixture was stirred until homogeneous and then placed in an ice-water bath for another two hours. This was designated as sample number one. Then, 1 g of ammonium persulfate was added to 20 mL of water and stirred until homogeneous. This was designated as sample number two. After stirring sample number one for two hours, solution number two was slowly added to it while stirring continuously. The mixture was stirred for another hour. The sample was then immediately centrifuged. It was washed twice with water and three times with ethanol, ensuring that the last wash was with ethanol. After washing, the sample was dried overnight in an oven at 75°C to obtain TiO2@PANI particles.
[0032] At room temperature, 0.15 g of TiO2@PANI sample was added to 1.5 mL of silicone oil and ground evenly in a mortar to obtain the required electrorheological fluid (weight ratio 10%). The electrorheological properties of the sample were then tested. Figure 7 The graph shows the relationship between shear stress and shear rate of the obtained electrorheological fluid under different electric field intensities. It can be seen from the graph that the shear stress does not increase significantly after applying an electric field. According to the electrorheological efficiency formula e = (η... E The calculation of -η0) / η0 yields the result at 2kV, 0.1s. -1 The current-rate efficiency was only 51.1%, which is far less than that of TiO2@PANI coated with 4ml aniline. The coating effect was poor, and good current-rate performance was not obtained.
[0033] Example 3 (Preparation of TiO2@PANI nanoparticles from 5 mL aniline)
[0034] Add 1.6 mL of hydrofluoric acid to 10 mL of acetic acid, stir continuously until homogeneous, then add 5 mL of TBT, continue stirring until homogeneous, and then transfer to a reaction vessel. Heat to 200°C for the first hydrothermal reaction for 12 hours. After the reaction is complete, allow the temperature to drop to room temperature, then centrifuge and wash, and place in an oven to dry overnight at 75°C. Dissolve 0.5 g of the solid sample obtained in the first step in 20 mL of ultrapure water, stir continuously until the solution is homogeneous, then transfer to a reaction vessel and heat to 120°C for the second hydrothermal reaction for 3 hours. After the reaction is complete, allow the temperature to drop to room temperature, then centrifuge and wash, and place in an oven to dry overnight at 75°C. The resulting titanium dioxide template is consistent with that obtained in Example 1, both being hollow cubic in shape. The solid sample obtained from the above reaction was dissolved in 100 mL of ethanol and stirred until homogeneous. While stirring, 0.1 g of CTAB, 5 mL of aniline, and 0.15 mL of acetic acid were added sequentially. The mixture was stirred until homogeneous and then placed in an ice-water bath for two hours. This was designated as sample number one. Then, 1 g of ammonium persulfate was added to 20 mL of water and stirred until homogeneous. This was designated as sample number two. After stirring sample number one for two hours, solution number two was slowly added to it while stirring continuously. The mixture was stirred for another hour. The sample was then immediately centrifuged. It was washed twice with water and three times with ethanol, ensuring that the last wash was with ethanol. After washing, the sample was dried overnight in an oven at 75°C to obtain TiO2@PANI particles.
[0035] At room temperature, 0.15 g of TiO2@PANI sample was added to 1.5 mL of silicone oil and ground evenly in a mortar to obtain the required electrorheological fluid (weight ratio 10%). The electrorheological properties of the sample were then tested. Figure 8 The graph shows the relationship between shear stress and shear rate for the obtained electrorheological fluid under different electric field intensities. It can be seen from the graph that the shear stress also increases significantly after the application of an electric field, but according to the electrorheological efficiency formula e = (η... E The calculation of -η0) / η0 yields the result at 3kV, 0.1s -1 The current-rate efficiency was only 59.8%, which is far less than that of TiO2@PANI coated with 4ml aniline. The coating effect was poor, and good current-rate performance was not obtained.
[0036] Example 4 (Preparation of TiO2@PANI nanoparticles from 6 mL aniline)
[0037] Add 1.6 mL of hydrofluoric acid to 10 mL of acetic acid, stir continuously until homogeneous, then add 5 mL of TBT, continue stirring until homogeneous, and then transfer to a reaction vessel. Heat to 200°C for the first hydrothermal reaction for 12 hours. After the reaction is complete, allow the temperature to drop to room temperature, then centrifuge and wash, and place in an oven to dry overnight at 75°C. Dissolve 0.5 g of the solid sample obtained in the first step in 20 mL of ultrapure water, stir continuously until the solution is homogeneous, then transfer to a reaction vessel and heat to 120°C for the second hydrothermal reaction for 3 hours. After the reaction is complete, allow the temperature to drop to room temperature, then centrifuge and wash, and place in an oven to dry overnight at 75°C. The resulting titanium dioxide template is consistent with that obtained in Example 1, both being hollow cubic in shape. The solid sample obtained from the above reaction was dissolved in 100 mL of ethanol and stirred until homogeneous. While stirring, 0.1 g of CTAB, 6 mL of aniline, and 0.2 mL of acetic acid were added sequentially. After stirring until homogeneous, the sample was placed in an ice-water bath and stirred for another two hours. This sample was designated as sample number one. Then, 1 g of ammonium persulfate was added to 20 mL of water and stirred until homogeneous. This sample was designated as sample number two. After stirring sample number one for two hours, sample number two was slowly added to it while stirring continuously. The stirring was continued for another hour. The sample was then immediately centrifuged. It was washed twice with water and three times with ethanol, ensuring that the last wash was with ethanol. After washing, the sample was dried overnight in an oven at 75°C to obtain TiO2@PANI particles. Figure 7 The image shows a scanning electron microscope (SEM) image of TiO2@PANI particles. The SEM image shows that polyaniline particles are uniformly coated on the surface of cubic titanium dioxide, and the coating effect is better and more obvious than that in Experiment 1. Figure 8 The image shows a transmission electron microscope (TEM) image of TiO2@PANI particles. The TEM image also reveals that the particles are hollow, maintaining a hollow structure. Furthermore, the transparency of the center decreases after coating, while the outer layer becomes darker, indicating a uniform coating layer. This confirms that the sample has a cubic hollow core-shell structure. Figure 9 The XRD pattern of TiO2@PANI particles shows the presence of anatase titanium dioxide and diffraction peaks of amorphous polyaniline, which proves that polyaniline has been coated on the surface of titanium dioxide.
[0038] At room temperature, 0.15 g of TiO2@PANI sample was added to 1.5 mL of silicone oil and ground evenly in a mortar to obtain the required electrorheological fluid (weight ratio 10%). The electrorheological properties of the sample were then tested. Figure 10 The graph shows the relationship between shear stress and shear rate of the obtained electrorheological fluid under different electric field intensities. It can be seen from the graph that the shear stress increases significantly after the application of an electric field. According to the electrorheological efficiency formula e = (η... E The calculation of -η0) / η0 yields the result at 3kV, 0.1s -1The current-rate efficiency was 485.3, with a larger variation range. It had a higher current-rate efficiency than TiO2@PANI coated with 4 ml aniline, and the coating effect was better, showing excellent current-rate performance.
Claims
1. A TiO2@PANI core-shell hollow cubic nanoparticle electrorheological fluid material, characterized in that... The dispersed phase of this electrorheological fluid material is a polyaniline-coated titanium dioxide core-shell hollow cubic nanoparticle, and the continuous phase is dimethyl silicone oil. Hollow cubic titanium dioxide nanoparticles are obtained through secondary hydrothermal treatment, and then polyaniline is coated onto their surface via in-situ polymerization at low temperature to prepare TiO2@PANI core-shell hollow cubic nanoparticles. These nanoparticles, with a hollow cubic titanium dioxide inner layer uniformly coated with polyaniline, exhibit a very distinct core-shell structure morphology, enhancing interfacial polarization. The electrorheological fluid formulated with these nanoparticles shows good electrorheological performance and low density. Hollow cubic titanium dioxide possesses anisotropy and porosity, while polyaniline exhibits good electrical conductivity, chemical stability, and a simple synthesis process. The preparation process includes the following steps: (1) Add 1.6 mL of hydrofluoric acid to 10 mL of acetic acid, stir continuously until uniform, then add 5 mL of TBT, continue stirring until uniform, and then put it into a reaction vessel. Heat to 200 °C for the first hydrothermal reaction for 12 h. After the reaction is complete, wait for the temperature to drop to room temperature, then centrifuge and wash the product, and put it in an oven to dry overnight at 75 °C. (2) Dissolve 0.5g of the solid sample obtained in the first step in 20mL of ultrapure water, stir continuously until the solution is mixed evenly, then put it into a reaction vessel, heat to 120℃ for a second hydrothermal reaction, and heat for 3h. After the reaction is completed, wait for the temperature to drop to room temperature, then centrifuge and wash the sample, and put it in an oven to dry overnight at 75℃; (3) Dissolve the solid sample obtained from the above reaction in 100 mL of ethanol, stir until homogeneous, and add 0.1 g CTAB, 6 mL aniline, and 0.2 mL acetic acid sequentially while stirring. Stir until homogeneous and place in an ice-water bath for two hours. This is recorded as sample number one. Then add 1 g ammonium persulfate to 20 mL of water and stir until homogeneous. This is recorded as sample number two. After stirring sample number one for two hours, slowly add solution number two while stirring continuously. Continue stirring for 1 hour. Then immediately centrifuge the sample, washing it twice with water and three times with ethanol, ensuring that the last wash is with ethanol. After washing, place the sample in an oven at 75 °C and dry overnight to obtain TiO2@PANI particles. (4) The sample was mixed with dimethyl silicone oil at a weight ratio of 10% to prepare an electrorheological fluid.
Citation Information
Patent Citations
Anisotropic titanium oxide / polyaniline nanocomposite electrorheological fluid and preparation method thereof
CN106010736A
Electrorheological fluid material of titanium dioxide cubic hollow nano particles and preparation method of electrorheological fluid material
CN110452765A