Nanometer metal particle dispersion strengthened copper alloy and preparation method thereof

By introducing nano-sized refractory metal particles into copper alloys, the problems of decreased electrical and thermal conductivity and complex preparation of traditional alumina dispersion-strengthened copper alloys have been solved, enabling the preparation of high-performance, low-cost copper alloys suitable for large-scale industrial production.

CN117947305BActive Publication Date: 2026-11-24UNIV OF SCI & TECH BEIJING
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410127747.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-30
Publication Date
2026-11-24
Estimated Expiration
2044-01-30

AI Technical Summary

Technical Problem

Traditional alumina dispersion-strengthened copper alloys are prone to the formation of large-sized Al₂O₃ particles and inclusions during the preparation process, which leads to a decrease in electrical and thermal conductivity. Furthermore, existing preparation methods suffer from problems such as impurity introduction, complex processes, high costs, and low efficiency.

Method used

High-performance copper alloys are prepared by replacing alumina with nano-refractory metal particles (such as W, Mo, Ta, Nb), preparing uniformly distributed nano-metal particles through chloride dissolution and high-energy ball milling, and then combining heat treatment and hot working methods.

Benefits of technology

Significant improvements in the tensile strength, electrical conductivity, and thermal conductivity of copper alloys have been achieved, resulting in good product performance consistency, suitability for mass production, and reduced costs and complexity.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention provides a copper alloy reinforced by nano-metal particle dispersion and its preparation method, relating to the technical field of copper alloy powder metallurgy. The nano-metal particle dispersion-reinforced copper alloy is a copper alloy in which nano-refractory metal particles are uniformly distributed within micron and submicron copper grains. The preparation method includes the preparation of copper@refractory metal chloride composite powder, mechanical alloying powder preparation, dispersion-reinforced copper alloy preparation, and plastic processing of the dispersion-reinforced copper alloy. This invention replaces aqueous solutions with organic solvents, replaces alumina dispersion reinforcement with refractory metal nanoparticle reinforcement, and combines this with hot working that allows for very large deformation. The prepared copper alloy, while maintaining excellent mechanical properties, exhibits superior electrical and thermal conductivity, high repeatability, low cost, and high efficiency. It eliminates the need for complex subsequent heat treatment and broadens its application range, facilitating large-scale industrial production and widespread use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of copper alloy powder metallurgy, and particularly to a copper alloy reinforced by nano-metal particle dispersion and its preparation method. Background Technology

[0002] Traditional dispersion-strengthened copper alloys are copper alloys reinforced by the dispersion of nano-sized alumina particles. They possess high strength, high hardness, and high wear resistance, while also exhibiting high electrical and thermal conductivity. More importantly, alumina dispersion-strengthened copper exhibits outstanding high-temperature performance, maintaining high strength even at 900℃ without significant changes in its microstructure. Therefore, alumina dispersion-strengthened copper demonstrates significant advantages in applications requiring high temperatures or undergoing high-temperature treatment.

[0003] However, the mainstream production process of traditional alumina dispersion-strengthened copper is to synthesize nano-alumina from Cu-Al alloy powder through internal oxidation. Due to the segregation of Al element in Cu-Al alloy powder and the large difference in diffusion rate between Al and O elements in the copper matrix, large submicron-sized Al2O3 particles are inevitably present in the dispersion-strengthened copper powder. In addition, large Al2O3 inclusions are often mixed in Cu-Al alloy powder, which makes the electrical and thermal conductivity of traditional alumina dispersion-strengthened copper decrease significantly. Cracking is prone to occur when drawing wires and stamping electrode caps, resulting in a low yield and limiting its large-scale application.

[0004] For example, Chinese patents CN108251685A, CN108356287A, and CN110184488A prepare tungsten dispersion-reinforced copper-based composite materials using sol-gel, catalytic gel, and spray pyrolysis methods, respectively. All three are aqueous solution chemical methods, and during the reduction of tungsten oxide, the hydrated oxide WO2(OH)2 may volatilize and condense, forming large-sized tungsten particles, which reduces the performance of the composite material. Chinese patent CN114293232A discloses a method for preparing tungsten dispersion-reinforced matrix composite materials using electroforming. Although this method can synthesize nano-tungsten particles to reinforce the copper matrix, the preparation process requires a large amount of electrical energy and has low production efficiency.

[0005] Chinese patent CN101487108A discloses a method for preparing a nano-dispersed phase reinforced copper alloy: the reinforcing element added to the copper alloy is selected from one or more of Ti, Co, P, Ni, Mg...Cr, Zr, Be or Fe, and the amount of reinforcing element added is 0.1-15% of the weight of the copper alloy. The tensile strength after the enhancement is far below 600MPa, and the thermal conductivity and electrical conductivity are poor.

[0006] Chinese patent CN116043052A discloses a nano-dispersion strengthened copper alloy and its preparation method and application. It is obtained by adding Cr powder to Cu-Al2O3 dispersed copper powder to obtain a composite powder, and then pressing, sintering, forming, hot extrusion, solution treatment, cold deformation and aging treatment. Obviously, it is an improvement on the traditional dispersion strengthened copper alloy, which increases the number of processes, reduces production efficiency and increases production cost.

[0007] Chinese patent CN111893343A discloses a modified nanoparticle dispersion-strengthened copper alloy and its preparation method. The modified nanoparticle dispersion-strengthened copper alloy includes copper and modified nanoparticles dispersed in the copper. The modified nanoparticles include nanoparticles and polydopamine coated on the surface of the nanoparticles. The nanoparticles are inorganic nanoparticles, which is obviously an improvement on the traditional dispersion-strengthened copper alloy. However, this preparation method has technical defects such as insignificant improvement in alloy performance, long process, and low efficiency. Summary of the Invention

[0008] The technical problem this invention aims to solve is that most current copper alloy strengthening methods rely on alumina dispersion strengthening, which leads to the formation of large alumina particles that affect the thermal and electrical conductivity of the copper alloy. Although there are copper-based composite materials strengthened by tungsten dispersion, the preparation method results in the technical defect of WO2(OH)2 volatilization and agglomeration, forming large-sized tungsten particles. Other methods mostly involve adding strengthening elements and inorganic nanoparticles to the copper alloy, but the preparation process introduces impurities, is complex, difficult to operate, costly, inefficient, and not conducive to industrial production.

[0009] To solve the above-mentioned technical problems, the present invention provides the following technical solution:

[0010] A copper alloy reinforced by nano-metal particle dispersion, wherein the copper alloy is a copper alloy in which nano-refractory metal particles are uniformly distributed within micron and submicron copper grains.

[0011] Preferably, the refractory metal nanoparticles are one or more of W, Mo, Ta, and Nb nanoparticles, and the size of the refractory metal nanoparticles is 5-20 nm.

[0012] Preferably, when the nano-refractory metal particles are W nano-metal particles, the tensile strength of the nano-metal particle dispersion-strengthened copper alloy is 652-775 MPa, the yield strength is 597-706 MPa, the elongation is 8-17%, the hardness is HRB75-90, the softening temperature is 850-950℃, the electrical conductivity is 82-91% IACS, and the thermal conductivity is 325-364 W·m. -1 ·k -1 ;

[0013] When the refractory metal nanoparticles are Mo nanoparticles, the tensile strength of the nanoparticle-dispersion-strengthened copper alloy is 669-835 MPa, the yield strength is 582-761 MPa, the elongation is 9-18%, the hardness is HRB78-93, the softening temperature is 850-950℃, the electrical conductivity is 83-90% IACS, and the thermal conductivity is 328-361 W·m. -1 ·k -1 ;

[0014] When the refractory metal nanoparticles are Ta nanoparticles, the tensile strength of the nanoparticle-dispersion-strengthened copper alloy is 642-753 MPa, the yield strength is 577-683 MPa, the elongation is 8-15%, the hardness is HRB72-88, the softening temperature is 830-950℃, the electrical conductivity is 83-89% IACS, and the thermal conductivity is 326-352 W·m. -1 ·k -1 ;

[0015] When the refractory metal nanoparticles are Nb nanoparticles, the tensile strength of the nanoparticle-dispersion-strengthened copper alloy is 685-852 MPa, the yield strength is 598-764 MPa, the elongation is 6-14%, the hardness is HRB80-95, the softening temperature is 850-950℃, the electrical conductivity is 81-87% IACS, and the thermal conductivity is 316-347 W·m. -1 ·k -1 .

[0016] A method for preparing a copper alloy reinforced by dispersion of the aforementioned nano-metal particles, the method comprising the following steps:

[0017] Preparation of S1, copper@refractory metal chloride composite powder

[0018] First, pure copper powder and refractory metal chloride are weighed in proportion as raw materials. Then, the chloride is dissolved in an organic solvent, and pure copper powder is added and stirred evenly. The organic solvent is then dried to obtain copper@chloride composite powder.

[0019] S2, Mechanical Alloying Powder Preparation

[0020] The copper@chloride composite powder of S1 was placed in a ball mill jar and ball milled until the chloride was completely dissolved into the copper matrix to obtain Cu-M-Cl mechanical alloying powder, wherein M is one or more of the refractory metals W, Mo, Ta and Nb.

[0021] S3, Preparation of Dispersion-Strengthened Copper Alloy Powder

[0022] S2 Cu-M-Cl mechanical alloying powder was placed in a hydrogen reduction furnace for heat treatment to obtain nano-metal particle dispersion-strengthened copper alloy powder.

[0023] S4, Preparation of Dispersion-Strengthened Copper Alloys

[0024] S3 nano-metal particle dispersion-strengthened copper alloy powder is formed into a green blank by molding or cold isostatic pressing, and then sintered to obtain a dispersion-strengthened copper alloy sintered blank.

[0025] S5, Dispersion-strengthened copper alloy plastic processing

[0026] By hot extrusion, hot rolling, or hot forging of the S4 dispersion-strengthened copper alloy sintered billet, fully dense, high-performance nano-metal particle dispersion-strengthened copper alloy products are obtained.

[0027] Preferably, the refractory metal in S1 accounts for 3-10% of the total mass of the refractory metal and copper.

[0028] Preferably, the pure copper powder in S1 is one or more of electrolytic copper powder, reduced copper powder, and atomized copper powder.

[0029] Preferably, the refractory metal chloride in S1 is one or more of WCl6, MoCl5, TaCl5, and NbCl5.

[0030] Preferably, the organic solvent in S1 is one or more of carbon disulfide, diethyl ether, ethanol, benzene, and carbon tetrachloride.

[0031] Preferably, in S2, the ball milling is carried out by one or more of the following methods: planetary ball milling, vibratory ball milling, and stirring ball milling, with a ball-to-material ratio of 5:1 to 20:1, and the milling time is 10-30 hours.

[0032] Preferably, the heat treatment in S3 is carried out in a hydrogen reduction furnace with a hydrogen flow rate of 0.5-5 L / min; the heat treatment is a two-stage heating and holding process: the first stage is heating to 150-400℃ and holding for 0.5-4 h; the second stage is heating to 500-800℃ and holding for 0.5-2 h.

[0033] Preferably, the pressing pressure in S4 is 100-600MPa, and the holding time is 30-300s; the green blank is heated to 900-1050℃ for sintering, and the holding time is 0.5-5h.

[0034] Preferably, the sintering method described in S4 is vacuum sintering or atmosphere-protected sintering, wherein the atmosphere-protected sintering is carried out by one or more of dry hydrogen, nitrogen, argon, methane, and acetylene.

[0035] Preferably, the preheating temperature for hot extrusion, hot rolling, or hot forging in S5 is 750-950°C, and the deformation is 60-98%.

[0036] Technical principle of the invention:

[0037] Studies have shown that the second phase responsible for dispersion strengthening consists of uniformly dispersed nanoparticles in the matrix, possessing high thermal stability and insoluble in the copper matrix. Based on this principle, refractory metals such as W, Mo, Ta, and Nb, which have no solid solubility in the copper matrix, can be nanoscaled and used as dispersion-strengthening second-phase particles. Furthermore, since the electrical and thermal conductivity of refractory metals is far superior to that of oxides such as alumina, copper alloys strengthened by dispersion using refractory metal nanoparticles exhibit better overall performance than traditional alumina-strengthened copper alloys.

[0038] The above technical solution has at least the following advantages compared with the existing technology:

[0039] The present invention proposes a method for preparing a nano-metal particle dispersion-strengthened copper alloy, which overcomes the technical defects of existing copper alloy preparation technologies, such as the introduction of impurities during the preparation process, complex procedures, high operational difficulty, high cost, low efficiency, significant decrease in electrical and thermal conductivity, difficulty in eliminating large alumina particles leading to poor processing performance, and other disadvantages to industrial production.

[0040] This invention obtains refractory metal nanoparticles through chlorides, avoiding the problem of refractory metal particle growth caused by the volatilization and agglomeration of hydrated oxides in other aqueous chemical preparation processes. This results in refractory metal nanoparticles with relatively uniform size and distribution in the copper matrix. The metal dispersion strengthened copper alloy products prepared in this way have high performance consistency and good product stability, and can be continuously drawn, stamped and other plastic processing, making them suitable for large-scale production.

[0041] This invention obtains Cu-M-Cl mechanically alloyed powder by high-energy ball milling of copper@chloride composite powder. The Cu-M-Cl mechanically alloyed powder can be heat-treated with hydrogen to obtain nano-metal particle dispersion-strengthened copper alloy powder for powder metallurgy preparation of copper alloys. It has low inclusion content and uniform dispersion distribution of nano-metal particles.

[0042] This invention obtains fully dense, high-performance nano-metal particle dispersion-strengthened copper alloy products by hot extrusion, hot rolling, or hot forging of dispersion-strengthened copper alloy sintered billets. The hot working deformation is very large, and the microstructure of the prepared copper alloy products is fine, which improves mechanical properties, thermal conductivity, and electrical conductivity.

[0043] According to current reports, the most superior common alumina dispersion-strengthened copper has an Al mass fraction of 0.6 wt.%, a tensile strength of 580 MPa, an electrical conductivity of 78% IACS, and a thermal conductivity of 305 W·m.-1 ·k -1 The preparation process provided by this invention results in significantly higher tensile strength, electrical conductivity, and thermal conductivity compared to alumina dispersion-strengthened copper, demonstrating significant advantages.

[0044] In summary, compared with other traditional methods, the method of this invention replaces the aqueous solution with an organic solvent, replaces the alumina dispersion reinforcement with refractory metal nanoparticle reinforcement, and combines it with hot working with a very large deformation to prepare copper alloys. The prepared copper alloys have better electrical and thermal conductivity while ensuring excellent mechanical properties. They are highly repeatable, low in cost, and highly efficient. They do not require complex subsequent heat treatment and have broadened the application range, which is conducive to large-scale industrial production and promotion. Detailed Implementation

[0045] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the described embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0046] A copper alloy reinforced by nano-metal particle dispersion, wherein the copper alloy is a copper alloy in which nano-refractory metal particles are uniformly distributed within micron and submicron copper grains.

[0047] Specifically, the nano-refractory metal particles are one or more of W, Mo, Ta, and Nb nano-metal particles, and the size of the nano-refractory metal particles is 5-20 nm.

[0048] Specifically, when the nano-refractory metal particles are W nano-metal particles, the tensile strength of the nano-metal particle dispersion-strengthened copper alloy is 652-775 MPa, the yield strength is 597-706 MPa, the elongation is 8-17%, the hardness is HRB75-90, the softening temperature is 850-950℃, the electrical conductivity is 82-91% IACS, and the thermal conductivity is 325-364 W·m. -1 ·k -1 ;

[0049] When the refractory metal nanoparticles are Mo nanoparticles, the tensile strength of the nanoparticle-dispersion-strengthened copper alloy is 669-835 MPa, the yield strength is 582-761 MPa, the elongation is 9-18%, the hardness is HRB78-93, the softening temperature is 850-950℃, the electrical conductivity is 83-90% IACS, and the thermal conductivity is 328-361 W·m. -1 ·k -1 ;

[0050] When the refractory metal nanoparticles are Ta nanoparticles, the tensile strength of the nanoparticle-dispersion-strengthened copper alloy is 642-753 MPa, the yield strength is 577-683 MPa, the elongation is 8-15%, the hardness is HRB72-88, the softening temperature is 830-950℃, the electrical conductivity is 83-89% IACS, and the thermal conductivity is 326-352 W·m. -1 ·k -1 ;

[0051] When the refractory metal nanoparticles are Nb nanoparticles, the tensile strength of the nanoparticle-dispersion-strengthened copper alloy is 685-852 MPa, the yield strength is 598-764 MPa, the elongation is 6-14%, the hardness is HRB80-95, the softening temperature is 850-950℃, the electrical conductivity is 81-87% IACS, and the thermal conductivity is 316-347 W·m. -1 ·k -1 .

[0052] A method for preparing a copper alloy reinforced by dispersion of the aforementioned nano-metal particles, the method comprising the following steps:

[0053] Preparation of S1, copper@refractory metal chloride composite powder

[0054] First, pure copper powder and refractory metal chloride are weighed in proportion as raw materials. Then, the chloride is dissolved in an organic solvent, and pure copper powder is added and stirred evenly. The organic solvent is then dried to obtain copper@chloride composite powder.

[0055] S2, Mechanical Alloying Powder Preparation

[0056] The copper@chloride composite powder of S1 was placed in a ball mill jar and ball milled until the chloride was completely dissolved into the copper matrix to obtain Cu-M-Cl mechanical alloying powder, wherein M is one or more of the refractory metals W, Mo, Ta and Nb.

[0057] S3, Preparation of Dispersion-Strengthened Copper Alloy Powder

[0058] S2 Cu-M-Cl mechanical alloying powder was placed in a hydrogen reduction furnace for heat treatment to obtain nano-metal particle dispersion-strengthened copper alloy powder.

[0059] S4, Preparation of Dispersion-Strengthened Copper Alloys

[0060] S3 nano-metal particle dispersion-strengthened copper alloy powder is formed into a green blank by molding or cold isostatic pressing, and then sintered to obtain a dispersion-strengthened copper alloy sintered blank.

[0061] S5, Dispersion-strengthened copper alloy plastic processing

[0062] By hot extrusion, hot rolling, or hot forging of the S4 dispersion-strengthened copper alloy sintered billet, fully dense, high-performance nano-metal particle dispersion-strengthened copper alloy products are obtained.

[0063] Specifically, refractory metals account for 3-10% of the total mass of refractory metals and copper in S1.

[0064] Specifically, the pure copper powder mentioned in S1 is one or more of electrolytic copper powder, reduced copper powder, and atomized copper powder.

[0065] Specifically, the refractory metal chloride mentioned in S1 is one or more of WCl6, MoCl5, TaCl5, and NbCl5.

[0066] Specifically, the organic solvent mentioned in S1 is one or more of carbon disulfide, diethyl ether, ethanol, benzene, and carbon tetrachloride.

[0067] Specifically, in S2, ball milling is carried out using one or more of the following methods: planetary ball milling, vibratory ball milling, and stirring ball milling, with a ball-to-material ratio of 5:1 to 20:1, and the milling time is 10-30 hours.

[0068] Specifically, the heat treatment in S3 is carried out in a hydrogen reduction furnace with a hydrogen flow rate of 0.5-5 L / min; the heat treatment consists of two stages of heating and holding: the first stage is heating to 150-400℃ and holding for 0.5-4 h; the second stage is heating to 500-800℃ and holding for 0.5-2 h.

[0069] Specifically, the pressing pressure in S4 is 100-600MPa, and the holding time is 30-300s; the green blank is heated to 900-1050℃ for sintering, and the holding time is 0.5-5h.

[0070] Specifically, the sintering method described in S4 is vacuum sintering or atmosphere-protected sintering, wherein the atmosphere-protected sintering is carried out by one or more of dry hydrogen, nitrogen, argon, methane, and acetylene.

[0071] Specifically, the preheating temperature for hot extrusion, hot rolling, or hot forging in S5 is 750-950℃, and the deformation is 60-98%.

[0072] Example 1

[0073] A W-nano metal particle dispersion-strengthened copper alloy, wherein the W-nano metal particle dispersion-strengthened copper alloy is a copper alloy in which W-nano refractory metal particles with an average size of 5 nm are uniformly distributed inside copper grains with an average grain size of 290 nm.

[0074] A method for preparing a copper alloy reinforced by W nano-metal particles dispersion, comprising the following steps:

[0075] Preparation of S1, copper@refractory metal chloride WCl6 composite powder

[0076] First, electrolytic copper powder and refractory metal chloride WCl6 are weighed as raw materials at a ratio of 3% of the total mass of refractory metal tungsten and copper. Then, refractory metal chloride WCl6 is dissolved in organic solvent carbon disulfide. Electrolytic copper powder is then added and stirred evenly. The organic solvent carbon disulfide is then dried to remove the carbon disulfide, resulting in copper@refractory metal chloride WCl6 composite powder with WCl6 uniformly coated on electrolytic copper powder.

[0077] S2, Mechanical Alloying Powder Preparation

[0078] The copper@refractory metal chloride WCl6 composite powder of S1 was placed in a ball mill jar for planetary ball milling with a ball-to-material ratio of 5:1 and a milling time of 30h. The refractory metal chloride WCl6 was completely dissolved into the copper matrix to obtain Cu-W-Cl mechanical alloying powder.

[0079] S3, Preparation of Dispersion-Strengthened Copper Alloy Powder

[0080] The Cu-W-Cl mechanical alloying powder of S2 was placed in a hydrogen reduction furnace for two-stage heating heat treatment. The hydrogen flow rate in the hydrogen reduction furnace was 0.5 L / min. The first stage was heated to 400℃ and held for 0.5 h. The second stage was heated to 500℃ and held for 2 h to obtain nano-metal particle dispersion-strengthened copper alloy powder.

[0081] S4, Preparation of Dispersion-Strengthened Copper Alloys

[0082] S3 nano-metal particle dispersion-strengthened copper alloy powder was formed into a green blank by cold isostatic pressing at a pressure of 100 MPa and a holding time of 300 s. The green blank was then heated to 900 °C under hydrogen atmosphere for atmosphere protection sintering and held for 0.5 h to obtain a dispersion-strengthened copper alloy sintered blank.

[0083] S5, Dispersion-strengthened copper alloy plastic processing

[0084] Hot extrusion was performed on the S4 dispersion-strengthened copper alloy sintered billet at a preheating temperature of 750℃ and a deformation amount of 98%, resulting in a fully dense, high-performance W nano-metal particle dispersion-strengthened copper alloy product.

[0085] The W nanoparticle-reinforced copper alloy prepared in this embodiment has a tensile strength of 652 MPa, a yield strength of 597 MPa, an elongation of 17%, a hardness of HRB75, a softening temperature of 850℃, an electrical conductivity of 91% IACS, and a thermal conductivity of 364 W·m. -1 ·k -1 .

[0086] Example 2

[0087] A Mo nanoparticle-reinforced copper alloy, wherein the Mo nanoparticle-reinforced copper alloy is a copper alloy in which Mo nanoparticles with an average size of 14 nm are uniformly distributed inside copper grains with an average grain size of 630 nm.

[0088] A method for preparing a copper alloy based on the aforementioned Mo nanoparticle dispersion strengthening, the method comprising the following steps:

[0089] Preparation of S1, copper@refractory metal chloride MoCl5 composite powder

[0090] First, reduced copper powder and refractory metal chloride MoCl5 are weighed as raw materials at a ratio of 6% of the total mass of refractory metal molybdenum and copper. Then, refractory metal chloride MoCl5 is dissolved in organic solvent diethyl ether, and then reduced copper powder is added and stirred evenly. The organic solvent diethyl ether is removed by drying to obtain copper@refractory metal chloride MoCl5 composite powder with MoCl5 uniformly coated with reduced copper powder.

[0091] S2, Mechanical Alloying Powder Preparation

[0092] The copper@refractory metal chloride MoCl5 composite powder of S1 was placed in a ball mill jar for planetary ball milling with a ball-to-material ratio of 20:1 and a milling time of 10h. The refractory metal chloride MoCl5 was completely dissolved into the copper matrix to obtain Cu-Mo-Cl mechanical alloying powder.

[0093] S3, Preparation of Dispersion-Strengthened Copper Alloy Powder

[0094] The Cu-Mo-Cl mechanically alloyed powder of S2 was placed in a hydrogen reduction furnace for two-stage heating heat treatment. The hydrogen flow rate in the hydrogen reduction furnace was 5L / min. The first stage was heated to 150℃ and held for 4h. The second stage was heated to 800℃ and held for 0.5h to obtain nano-metal particle dispersion-strengthened copper alloy powder.

[0095] S4, Preparation of Dispersion-Strengthened Copper Alloys

[0096] S3 nano-metal particle dispersion-strengthened copper alloy powder was used to prepare green blanks by cold isostatic pressing at a pressure of 600 MPa for 30 s. The green blanks were then vacuum sintered at 1050 °C under hydrogen atmosphere with a vacuum degree of 10. -3 Pa, with a holding time of 3 hours, yielded a dispersion-strengthened copper alloy sintered billet;

[0097] S5, Dispersion-strengthened copper alloy plastic processing

[0098] The S4 dispersion-strengthened copper alloy sintered billet was hot-rolled at a preheating temperature of 950℃ and a deformation of 60% to obtain a fully dense, high-performance Mo nanoparticle dispersion-strengthened copper alloy product.

[0099] The Mo nanoparticle-reinforced copper alloy prepared in this embodiment has a tensile strength of 681 MPa, a yield strength of 615 MPa, an elongation of 13%, a hardness of HRB85, a softening temperature of 900℃, an electrical conductivity of 86% IACS, and a thermal conductivity of 347 W·m. -1 ·k -1 .

[0100] Example 3

[0101] A Ta nanoparticle dispersion-strengthened copper alloy, wherein the Ta nanoparticle dispersion-strengthened copper alloy is a copper alloy in which Ta nanoparticles of refractory metal with an average size of 20 nm are uniformly distributed inside copper grains with an average grain size of 820 nm.

[0102] A method for preparing a copper alloy based on the aforementioned Ta nanoparticle dispersion reinforcement, the method comprising the following steps:

[0103] Preparation of S1, copper@refractory metal chloride TaCl5 composite powder

[0104] First, atomized copper powder and refractory metal chloride TaCl5 are weighed as raw materials at a ratio of 10% of the total mass of refractory metal tantalum and copper. Then, refractory metal chloride TaCl5 is dissolved in organic solvent carbon tetrachloride. Next, atomized copper powder is added and stirred evenly. The organic solvent carbon tetrachloride is then dried to remove the carbon tetrachloride, resulting in copper@refractory metal chloride TaCl5 composite powder with TaCl5 uniformly coated on atomized copper powder.

[0105] S2, Mechanical Alloying Powder Preparation

[0106] The copper@refractory metal chloride TaCl5 composite powder of S1 was placed in a ball mill jar and subjected to planetary ball milling with a ball-to-material ratio of 10:1 and a milling time of 16h. The refractory metal chloride TaCl5 was completely dissolved into the copper matrix to obtain Cu-Ta-Cl mechanical alloying powder.

[0107] S3, Preparation of Dispersion-Strengthened Copper Alloy Powder

[0108] The Cu-Ta-Cl mechanical alloying powder of S2 was placed in a hydrogen reduction furnace for two-stage heating heat treatment. The hydrogen flow rate in the hydrogen reduction furnace was 2L / min. The first stage was heated to 240℃ and held for 2h. The second stage was heated to 600℃ and held for 1h to obtain nano-metal particle dispersion-strengthened copper alloy powder.

[0109] S4, Preparation of Dispersion-Strengthened Copper Alloys

[0110] S3 nano-metal particle dispersion-strengthened copper alloy powder was molded into a green blank by compression molding at a pressure of 400 MPa and a holding time of 120 s. The green blank was then heated to 950 °C under nitrogen atmosphere for atmosphere protection sintering and held for 2 h to obtain a dispersion-strengthened copper alloy sintered blank.

[0111] S5, Dispersion-strengthened copper alloy plastic processing

[0112] Hot extrusion was performed on the S4 dispersion-strengthened copper alloy sintered billet, with a preheating temperature of 850℃ and a deformation amount of 85%, to obtain a fully dense, high-performance Ta nano-metal particle dispersion-strengthened copper alloy product.

[0113] The Ta nanoparticle-reinforced copper alloy prepared in this embodiment has a tensile strength of 753 MPa, a yield strength of 683 MPa, an elongation of 8%, a hardness of HRB88, a softening temperature of 950℃, an electrical conductivity of 83% IACS, and a thermal conductivity of 326 W·m. -1 ·k -1 .

[0114] Example 4

[0115] A copper alloy reinforced by Nb nano-metal particles dispersion, wherein the copper alloy is a copper alloy in which Nb nano-refractory metal particles with an average size of 12 nm are uniformly distributed inside copper grains with an average grain size of 482 nm.

[0116] A method for preparing a copper alloy based on the aforementioned Nb nanoparticle dispersion reinforcement, the method comprising the following steps:

[0117] Preparation of S1, copper@refractory metal chloride NbCl5 composite powder

[0118] First, atomized copper powder and refractory metal chloride NbCl5 are weighed as raw materials at a ratio of 10% of the total mass of refractory metal tungsten and refractory metal niobium and copper. Then, refractory metal chloride NbCl5 is dissolved in organic solvent ethanol, and atomized copper powder is added and stirred evenly. The organic solvent ethanol is then removed by drying to obtain copper@refractory metal chloride NbCl5 composite powder with NbCl5 uniformly coated on atomized copper powder.

[0119] S2, Mechanical Alloying Powder Preparation

[0120] The copper@refractory metal chloride NbCl5 composite powder of S1 was placed in a ball mill jar for planetary ball milling with a ball-to-material ratio of 20:1 and a milling time of 20h. The refractory metal chloride NbCl5 was completely dissolved into the copper matrix to obtain Cu-Nb-Cl mechanical alloying powder.

[0121] S3, Preparation of Dispersion-Strengthened Copper Alloy Powder

[0122] The Cu-Nb-Cl mechanical alloying powder of S2 was placed in a hydrogen reduction furnace for two-stage heating heat treatment. The hydrogen flow rate in the hydrogen reduction furnace was 1L / min. The first stage was heated to 200℃ and held for 1h. The second stage was heated to 650℃ and held for 2h to obtain nano-metal particle dispersion-strengthened copper alloy powder.

[0123] S4, Preparation of Dispersion-Strengthened Copper Alloys

[0124] S3 nano-metal particle dispersion-strengthened copper alloy powder was molded into a green blank by compression molding at a pressure of 450 MPa and a holding time of 90 s. The green blank was then heated to 980 °C under argon atmosphere for atmosphere protection sintering and held for 3 h to obtain a dispersion-strengthened copper alloy sintered blank.

[0125] S5, Dispersion-strengthened copper alloy plastic processing

[0126] Hot extrusion was performed on the S4 dispersion-strengthened copper alloy sintered billet, with a preheating temperature of 900℃ and a deformation amount of 90%, to obtain a fully dense, high-performance Nb nano-metal particle dispersion-strengthened copper alloy product.

[0127] The Nb nanoparticle-reinforced copper alloy prepared in this embodiment has a tensile strength of 852 MPa, a yield strength of 764 MPa, an elongation of 6%, a hardness of HRB95, a softening temperature of 950 °C, an electrical conductivity of 81% IACS, and a thermal conductivity of 316 W·m. -1 ·k -1 .

[0128] The present invention proposes a method for preparing a nano-metal particle dispersion-strengthened copper alloy, which overcomes the technical defects of existing copper alloy preparation technologies, such as the introduction of impurities during the preparation process, complex procedures, high operational difficulty, high cost, low efficiency, significant decrease in electrical and thermal conductivity, difficulty in eliminating large alumina particles leading to poor processing performance, and other disadvantages to industrial production.

[0129] This invention obtains refractory metal nanoparticles through chlorides, avoiding the problem of refractory metal particle growth caused by the volatilization and agglomeration of hydrated oxides in other aqueous chemical preparation processes. This results in refractory metal nanoparticles with relatively uniform size and distribution in the copper matrix. The metal dispersion strengthened copper alloy products prepared in this way have high performance consistency and good product stability, and can be continuously drawn, stamped and other plastic processing, making them suitable for large-scale production.

[0130] This invention obtains Cu-M-Cl mechanically alloyed powder by high-energy ball milling of copper@chloride composite powder. The Cu-M-Cl mechanically alloyed powder can be heat-treated with hydrogen to obtain nano-metal particle dispersion-strengthened copper alloy powder for powder metallurgy preparation of copper alloys. It has low inclusion content and uniform dispersion distribution of nano-metal particles.

[0131] This invention obtains fully dense, high-performance nano-metal particle dispersion-strengthened copper alloy products by hot extrusion, hot rolling, or hot forging of dispersion-strengthened copper alloy sintered billets. The hot working deformation is very large, and the microstructure of the prepared copper alloy products is fine, which improves mechanical properties, thermal conductivity, and electrical conductivity.

[0132] According to current reports, the most superior common alumina dispersion-strengthened copper has an Al mass fraction of 0.6 wt.%, a tensile strength of 580 MPa, an electrical conductivity of 78% IACS, and a thermal conductivity of 305 W·m. -1 ·k -1 The preparation process provided by this invention results in significantly higher tensile strength, electrical conductivity, and thermal conductivity compared to alumina dispersion-strengthened copper, demonstrating significant advantages.

[0133] In summary, compared with other traditional methods, the method of this invention replaces the aqueous solution with an organic solvent, replaces the alumina dispersion reinforcement with refractory metal nanoparticle reinforcement, and combines it with hot working with a very large deformation to prepare copper alloys. The prepared copper alloys have better electrical and thermal conductivity while ensuring excellent mechanical properties. They are highly repeatable, low in cost, and highly efficient. They do not require complex subsequent heat treatment and have broadened the application range, which is conducive to large-scale industrial production and promotion.

[0134] The above description represents the preferred embodiments of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A copper alloy reinforced by nano-metal particle dispersion, characterized in that, The nano-metal particle dispersion-strengthened copper alloy is a copper alloy in which nano-refractory metal particles are uniformly distributed inside micron and submicron copper grains. The nano-refractory metal particles are one or more of W, Mo, Ta, and Nb, and the size of the nano-refractory metal particles is 5-20 nm. The preparation method of the aforementioned nano-metal particle dispersion-strengthened copper alloy is as follows: Preparation of S1, copper@refractory metal chloride composite powder First, pure copper powder and refractory metal chloride are weighed as raw materials in a certain proportion, with the refractory metal accounting for 3-10% of the total mass of the refractory metal and copper. Then, the chloride is dissolved in an organic solvent, and pure copper powder is added and stirred evenly. The organic solvent is then dried to obtain copper@chloride composite powder. S2, Mechanical Alloying Powder Preparation The copper@chloride composite powder of S1 was placed in a ball mill jar and ball milled until the chloride was completely dissolved into the copper matrix to obtain Cu-M-Cl mechanical alloying powder, wherein M is one or more of the refractory metals W, Mo, Ta and Nb. S3, Preparation of Dispersion-Strengthened Copper Alloy Powder S2 Cu-M-Cl mechanical alloying powder was placed in a hydrogen reduction furnace for heat treatment to obtain nano-metal particle dispersion-strengthened copper alloy powder. S4, Preparation of Dispersion-Strengthened Copper Alloys S3 nano-metal particle dispersion-strengthened copper alloy powder is formed into a green blank by molding or cold isostatic pressing, and then sintered to obtain a dispersion-strengthened copper alloy sintered blank. S5, Dispersion-strengthened copper alloy plastic processing By hot extrusion, hot rolling, or hot forging of the S4 dispersion-strengthened copper alloy sintered billet, fully dense, high-performance nano-metal particle dispersion-strengthened copper alloy products are obtained.

2. A method for preparing a copper alloy reinforced by dispersion of nano-metal particles according to claim 1, characterized in that, The preparation method includes the following steps: Preparation of S1, copper@refractory metal chloride composite powder First, pure copper powder and refractory metal chloride are weighed in proportion as raw materials. Then, the chloride is dissolved in an organic solvent, and pure copper powder is added and stirred evenly. The organic solvent is then dried to obtain copper@chloride composite powder. S2, Mechanical Alloying Powder Preparation The copper@chloride composite powder of S1 was placed in a ball mill jar and ball milled until the chloride was completely dissolved into the copper matrix to obtain Cu-M-Cl mechanical alloying powder, wherein M is one or more of the refractory metals W, Mo, Ta and Nb. S3, Preparation of Dispersion-Strengthened Copper Alloy Powder S2 Cu-M-Cl mechanical alloying powder was placed in a hydrogen reduction furnace for heat treatment to obtain nano-metal particle dispersion-strengthened copper alloy powder. S4, Preparation of Dispersion-Strengthened Copper Alloys S3 nano-metal particle dispersion-strengthened copper alloy powder is formed into a green blank by molding or cold isostatic pressing, and then sintered to obtain a dispersion-strengthened copper alloy sintered blank. S5, Dispersion-strengthened copper alloy plastic processing By hot extrusion, hot rolling, or hot forging of the S4 dispersion-strengthened copper alloy sintered billet, fully dense, high-performance nano-metal particle dispersion-strengthened copper alloy products are obtained.

3. The method for preparing nano-metal particle dispersion-strengthened copper alloy according to claim 2, characterized in that, The organic solvent mentioned in S1 is one or more of carbon disulfide, diethyl ether, ethanol, benzene, and carbon tetrachloride.

4. The method for preparing nano-metal particle dispersion-strengthened copper alloy according to claim 2, characterized in that, In S2, ball milling is carried out using one or more of the following methods: planetary ball milling, vibratory ball milling, and stirring ball milling, with a ball-to-material ratio of 5:1 to 20:1, and the milling time is 10-30 hours.

5. The method for preparing nano-metal particle dispersion-strengthened copper alloy according to claim 2, characterized in that, In S3, the heat treatment is carried out in a hydrogen reduction furnace with a hydrogen flow rate of 0.5-5 L / min. The heat treatment consists of two stages of heating and holding: the first stage is heating to 150-400℃ and holding for 0.5-4 h; the second stage is heating to 500-800℃ and holding for 0.5-2 h.

6. The method for preparing nano-metal particle dispersion-strengthened copper alloy according to claim 2, characterized in that, The pressing pressure for forming in S4 is 100-600MPa, and the holding time is 30-300s; the green blank is heated to 900-1050℃ for sintering, and the holding time is 0.5-5h.

7. The method for preparing nano-metal particle dispersion-strengthened copper alloy according to claim 2, characterized in that, The preheating temperature for hot extrusion, hot rolling, or hot forging in S5 is 750-950℃, and the deformation is 60-98%.

Citation Information

Patent Citations

  • Preparation of nano dispersed phase reinforced copper alloy

    CN101487108A

  • Method for preparing tungsten dispersion-strengthened copper-based composite material through gel catalyzing

    CN108356287A

  • Modified nanoparticle dispersion strengthened copper alloy, preparation method and application thereof, electronic element and mechanical element

    CN111893343A

  • Method for preparing tungsten dispersion strengthened copper composite material through electroforming

    CN114293232A

  • Nano dispersion strengthened copper alloy and preparation method and application thereof

    CN116043052A