165 ksi grade oil casing and quenching and partitioning heat treatment method thereof
By using thermoelectric quenching and bainization partitioning heat treatment methods to regulate the microstructure of martensite and carbide-free bainite, 165ksi grade oil casing was prepared, solving the high strength and high toughness requirements of deep and ultra-deep well oil and gas extraction and realizing the mass production of high-performance oil casing.
Patent Information
- Application Number
- CN202410103806.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-25
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-01-25
AI Technical Summary
Existing technologies are insufficient to meet the high strength and high toughness requirements of oil casing during deep and ultra-deep oil and gas resource extraction. Conventional API well tubing cannot meet the performance requirements of deep and ultra-deep wells, and the impact energy of steel-grade materials in existing patented processes is low or the composition varies significantly.
By combining the characteristics of martensite and carbide-free bainite, and employing thermothermal quenching and bainization partitioning heat treatment methods, the content of martensite and carbide-free bainite in the microstructure is controlled to prepare 165ksi grade oil casing, achieving a balance between high strength and high toughness.
We have produced high-strength and high-toughness 165ksi oil casing with a yield strength ≥1180MPa, tensile strength ≥1350MPa, elongation after fracture ≥16%, and transverse impact energy ≥100J. This has solved the problems of high residual stress and unstable performance of steel pipes, and achieved a balance between high strength and toughness.
Smart Images

Figure CN117947351B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of steel grade material preparation technology, and more specifically, it relates to a 165ksi steel grade oil casing and its quenching, bainizing, and partitioning heat treatment method. Background Technology
[0002] As industrial development progresses, oil and natural gas resources are continuously consumed, and the relatively easy-to-extract shallow oil and gas resources are gradually failing to meet development needs. Therefore, there is an urgent need to exploit deep and ultra-deep oil and gas resources. Deep and ultra-deep wells typically operate in harsher high-temperature and high-pressure environments. In some oil and gas fields, the bottom-hole temperature exceeds 200°C, and the wellbore pressure reaches 100 MPa. Furthermore, phenomena such as mudstone creep and rock slippage are prone to occur in deep geological formations, leading to more complex stress states for the casing and tubing during service. As essential equipment supporting the rock face, the casing and tubing, operating in such harsh environments, require new performance requirements in terms of strength and toughness to ensure safety during drilling operations.
[0003] Currently, oil casing production typically follows the American Petroleum Institute (API) standards. However, conventional API oil well tubing cannot meet the strength and toughness requirements of deep and ultra-deep well operations, leading to a growing demand for non-API tubing. To adapt to the unique operating environments of deep and ultra-deep wells and ensure safe production, there is an urgent need for the mass production and application of high-strength and high-toughness oil casing tubing made of 165ksi steel.
[0004] The patent (application number CN201710926992.4) discloses a low alloy steel for producing 170ksi grade steel pipes. After quenching and tempering, the tensile strength is ≥1250MPa, the yield strength is 1175-1265MPa, and the transverse full-size impact energy of Charpy U-notch at 0℃ is ≥80J. The low alloy steel produced by this process has high strength, but its impact energy is low.
[0005] Patent (application number CN202111540297.7) discloses a high-strength niobium-containing oil casing based on controlled cooling and its preparation method. The casing product has a yield strength of 1180-1300MPa and a tensile strength of 1250-1450MPa. The material microstructure consists of bainite, ferrite, and pearlite, which is significantly different from the carbide-free bainite / martensite composite microstructure in this technical route.
[0006] Patent (application number CN202310644746.5) discloses a method for producing 160ksi grade high-strength and high-toughness oil casing. The method produces 160ksi steel with a yield strength Rt0.7 ≥ 1110 MPa, a tensile strength Rm ≥ 1110 MPa, and Charpy V-type transverse and longitudinal impact energy greater than 110 J and 120 J at 0℃, respectively. The method involves the addition of Cu, Ti, and 0.05-0.35 wt.% Si, which is significantly different from the method in this invention, which does not include Cu, Ti, and Si and has a content of 1.00-2.00 wt.%. Summary of the Invention
[0007] This disclosure provides a 165ksi grade oil casing and its quenching and bainization heat treatment method, which solves the technical problem of poor toughness matching in high-strength steel by combining the characteristics of martensite and carbide-free bainite.
[0008] In a first aspect, this disclosure provides a 165ksi grade oil casing material, comprising the following components: C: 0.12-0.30 wt.%; Si: 1.00-2.00 wt.%; Mn: 1.50-2.40 wt.%; Cr: 1.00-2.00 wt.%; Mo: 0.50-1.50 wt.%; Nb: 0.03-0.06 wt.%, wherein: P≤0.020 wt.% and S≤0.020 wt.%, the remainder being Fe and other unavoidable impurity elements, by mass percentage.
[0009] Secondly, this disclosure provides a 165ksi grade oil casing and its quenching and bainizing heat treatment method, comprising the following steps:
[0010] Step 1: Dithermal quenching treatment transforms the steel pipe's microstructure into martensite while retaining some supercooled austenite.
[0011] Step 2: Bainification and partitioning treatment, which transforms the supercooled austenite in Step 1 into a carbide-free bainite structure and realizes the partitioning of carbon atoms in martensite into austenite;
[0012] Step 3: Slow cooling treatment, the steel pipe after step 2 is subjected to slow cooling treatment.
[0013] Preferably, the martensitic transformation start temperature Ms, the martensitic transformation end temperature Mf, and the bainitic transformation start temperature Bs of the steel pipe material are determined before step 1.
[0014] Preferably, the steel pipe rolling process is completed before step 1, and the final rolling temperature of the steel pipe is 900-980℃.
[0015] Preferably, step 1, the intermediate-temperature quenching treatment, includes: quenching the steel pipe at a rate greater than the critical martensitic cooling rate, to a cooling temperature of T1; T1 is between T1 and T2. 11 -T 12 Between, where T 11 =Mf+50 and T 12 =Ms-30.
[0016] Preferably, the shale-based distribution process in step 2 includes: heating the quenched steel pipe from temperature T1 to T2 and holding it at that temperature for a time of t (min);
[0017] Heating temperature T2 at T 21 -T 22 Between, where T 21 =Ms+10,T 22 =Ms+0.8*(Bs-Ms), where t is 5-10 times the millimeter wall thickness d of the steel pipe.
[0018] Preferably, the heating temperature T 22 At least 40°C below the Bs temperature.
[0019] Preferably, the slow cooling process in step 3 includes: cooling the steel pipe to room temperature under air cooling and wind cooling conditions, with an average cooling rate C (°C / s) between Bs / 500 and Bs / 60 per second.
[0020] Thirdly, this disclosure provides an application of 165ksi grade oil casing, wherein the yield strength R of the oil casing is... p0.2 ≥1180MPa, tensile strength R m ≥1350MPa, elongation after fracture A≥16%, transverse impact energy (0℃) A kv ≥100J.
[0021] The quenching and bainization heat treatment method of this application involves a partial martensitic phase transformation during the dielectric quenching stage, while retaining a portion of the supercooled austenite. During the bainization stage, the supercooled austenite retained undergoes a carbide-free bainite transformation, resulting in a carbide-free bainite / martensite composite structure. Furthermore, carbon atom distribution is completed at this stage, stabilizing the retained austenite and improving impact toughness, thereby obtaining a high-strength and high-toughness 165ksi oil casing product.
[0022] Generally, a high martensite content can significantly improve the strength of steel, but at the same time, it will greatly reduce toughness. Carbide-free bainitic microstructure, on the other hand, possesses both good strength and toughness. Therefore, in this invention, by controlling the appropriate martensite and carbide-free bainite content through the matching of composition and process, a high-strength and high-toughness oil casing of 165ksi grade steel with a carbide-free bainite / martensite composite microstructure is produced. Using the process method of this invention, mass production of 165ksi grade oil casing can be achieved.
[0023] In summary, this application has the following beneficial effects:
[0024] 1. The high martensite content in this application can significantly improve the strength of steel, but at the same time, it will greatly reduce the toughness. In contrast, the carbide-free bainitic structure combines good strength and toughness. Furthermore, it helps to solve the problems of high residual stress, poor precision, and poor performance stability in steel pipes.
[0025] 2. In this application, the appropriate content of martensite and carbide-free bainite is controlled by matching the composition and process to produce a high-strength and high-toughness matching oil casing of 165ksi steel grade with a carbide-free bainite / martensite composite structure, which has stable performance and product dimensions.
[0026] It should be understood that the above general description and the following detailed description are exemplary and explanatory only, and do not limit the scope of protection of this disclosure. Attached Figure Description
[0027] Figure 1 This is the microstructure of the 165ksi oil casing in Embodiment 1 of this application. Detailed Implementation
[0028] The following detailed description of this application is provided in conjunction with the embodiments. It should be noted that: unless otherwise specified, the conditions in the following embodiments are performed under conventional conditions or conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following embodiments are all from commercially available sources.
[0029] Example
[0030] The 165ksi oil casing of this application comprises the following material: C: 0.12-0.30 wt.%; Si: 1.00-2.00 wt.%; Mn: 1.50-2.40 wt.%; Cr: 1.00-2.00 wt.%; Ni: 1.00-1.50 wt.%; Mo: 0.50-1.50 wt.%; Nb: 0.03-0.06 wt.%. Wherein, P ≤ 0.020 wt.% and S ≤ 0.020 wt.%, with the remainder being Fe and other unavoidable impurity elements, by mass percentage.
[0031] Among them, C element: Increasing the C content is beneficial to improving the strength of the material, but excessively high C content will reduce the impact performance of the material. In this invention, the C content is reduced, and the content range is set at 0.12-0.30 wt.%. Si element: Si can shift the C curve to the right, inhibit the precipitation of brittle carbides, and is conducive to the formation of carbide-free bainite. Mn element: Delays high-temperature transformation, inhibits the formation of soft phase structures such as proeutectoid ferrite in oil casing products during slow cooling, which is conducive to obtaining bainite structure with good performance, and also has the effect of solid solution strengthening and stabilizing retained austenite. Cr element: Has a good solid solution strengthening effect, can significantly improve strength, and can significantly improve the hardenability of steel. Ni element: Can expand the austenite phase region, improve the stability of retained austenite in steel after quenching to increase its content, thereby improving the impact toughness of the material. Mo element: Increases the tempering temperature of steel, and can form carbide precipitates to improve the strength of steel. Nb element: can significantly refine the microstructure, and Nb is a carbide-forming element. The formed carbides play a role in precipitation strengthening, while improving the strength and toughness of the material.
[0032] The post-rolling quenching and bainization heat treatment process mainly consists of three steps: Step 1, thermothermal quenching, which transforms part of the steel pipe's microstructure into martensite while retaining some supercooled austenite; Step 2, bainization treatment, which transforms the supercooled austenite in Step 1 into carbide-free bainite and distributes carbon atoms from the martensite into the austenite; Step 3, slow cooling treatment, in which the steel pipe after Step 2 is slowly cooled to obtain a 165ksi oil casing with a carbide-free bainite / martensite composite microstructure.
[0033] In a preferred embodiment, the 244.48*11.99mm specification oil casing is selected and subjected to quenching and baining heat treatment after rolling. The preferred method is as follows:
[0034] Using relevant equipment, Bs = 470℃, Ms = 352℃, and Mf = 175℃ were measured. Bs, Ms, and Mf represent the bainitic transformation start temperature, martensitic transformation start temperature, and martensitic transformation end temperature, respectively.
[0035] Step 1, thermothermal quenching treatment: The steel pipe is quenched at a rate greater than the critical martensitic cooling rate until the cooling temperature reaches T1, where T1 is between T1 and T2. 11 -T 12 Between, where T 11 =Mf+50=225℃ and T 12 =Ms-30=322℃.
[0036] T1 can be, but is not limited to, 230℃, 250℃, 270℃, 290℃, and 310℃.
[0037] Step 2, shale-based fractionation treatment: The quenched steel pipe is heated from temperature T1 to T2 and held at that temperature for a time t (min). The heating temperature T2 is within the range of T... 21 -T 22 Between, where T 21 =Ms+10=362℃, T 22 =Ms+0.8*(Bs-Ms)=446.4℃, where t is 5-10 times the millimeter wall thickness d of the steel pipe;
[0038] T2 can be, but is not limited to, 370℃, 380℃, 390℃, 400℃, 410℃, and 420℃; t can be, but is not limited to, 65min, 75min, 85min, 95min, 105min, and 115min.
[0039] Step 3, slow cooling treatment, the steel pipe is cooled to room temperature under air cooling and wind cooling conditions, the average cooling rate C (°C / s) per second is between C1 and C2, where C1 = Bs / 500, C2 = Bs / 60.
[0040] C can be, but is not limited to, 1℃ / s, 2℃ / s, 3℃ / s, 4℃ / s, 5℃ / s, 6℃ / s, 7℃ / s
[0041] To more clearly illustrate the present invention, the invention will be further described below with reference to embodiments and accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0042] Tables 1 and 2 list the preferred chemical composition (mass percentage) and heat treatment process parameters for 165ksi grade oil casing in Examples 1-4, respectively. Table 3 shows the test results of mechanical properties.
[0043] Table 1. Mass percentage of chemical elements (wt.%)
[0044] serial number C Si Mn Cr Ni Mo Nb Example 1 0.12 1.95 2.26 1.90 1.15 1.41 0.05 Example 2 0.30 1.35 2.40 1.01 1.48 0.60 0.03 Example 3 0.22 1.28 2.02 1.20 1.42 0.89 0.05 Example 4 0.16 1.44 2.10 1.68 1.22 1.08 0.04
[0045] Table 2 Heat treatment process parameters
[0046] serial number <![CDATA[T1(℃)]]> <![CDATA[T2(℃)]]> t(min) C (°C / s) Example 1 300 420 70 2 Example 2 270 380 100 7 Example 3 310 400 65 1 Example 4 230 370 90 5
[0047] Table 3 Mechanical Properties of Oil Casing and Pipe
[0048]
[0049] As can be seen from the mechanical property test results shown in Table 3, the yield strength R of the 165ksi oil casing in Examples 1-4 is...p0.2 ≥1180MPa, tensile strength R m ≥1350MPa, elongation after fracture A≥16%, transverse impact energy (0℃) A kv ≥100J.
[0050] The above description is merely an exemplary embodiment of this disclosure, but the scope of protection of this disclosure is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this disclosure should be included within the scope of protection of this disclosure. Therefore, the scope of protection of this disclosure should be determined by the scope of the claims.
Claims
1. A quenching and baining heat treatment method for 165ksi grade oil casing, characterized in that, Includes the following steps: Step 1: Dithermal quenching treatment transforms the steel pipe's microstructure into martensite while retaining some supercooled austenite. Step 2: Bainification and partitioning treatment, which transforms the supercooled austenite in Step 1 into a carbide-free bainite structure and realizes the partitioning of carbon atoms in martensite into austenite; Step 3: Slow cooling treatment, the steel pipe after step 2 is subjected to slow cooling treatment; The 165ksi grade oil casing material comprises the following components: C: 0.12-0.30wt.%; Si: 1.00-2.00wt.%; Mn: 1.50-2.40wt.%; Cr: 1.00-2.00wt.%; Mo: 0.50-1.50wt.%; Nb: 0.03-0.06wt.%, wherein: P≤0.020wt.% and S≤0.020wt.%, and the remainder is Fe and other unavoidable impurity elements, by mass percentage; Before step 1, the martensitic transformation start temperature Ms, the martensitic transformation end temperature Mf, and the bainitic transformation start temperature Bs of the steel pipe material are determined. Step 1, the intermediate-temperature quenching treatment, includes: quenching the steel pipe at a rate greater than the critical martensitic cooling rate, to a cooling temperature of T1; T1 is between T1 and T2. 11 -T 12 Between, where T 11 =Mf+50 and T 12 =Ms-30; Step 2, the shale-based fractionation process, includes: heating the quenched steel pipe from temperature T1 to T2 and holding it at that temperature for a time t (min); the heating temperature T2 is within T... 21 -T 22 Between, where T 21 =Ms+10,T 22 =Ms+0.8*(Bs-Ms), where t is 5-10 times the millimeter wall thickness d of the steel pipe; The slow cooling process in step 3 includes cooling the steel pipe to room temperature under air cooling and wind cooling conditions, with an average cooling rate C (°C / s) between Bs / 500 and Bs / 60 per second.
2. The quenching and baining heat treatment method for 165ksi grade oil casing according to claim 1, characterized in that, The steel pipe rolling process is completed before step 1, and the final rolling temperature of the steel pipe is 900-980℃.
3. The quenching and baining heat treatment method for 165ksi grade oil casing according to claim 1, characterized in that, The heating temperature T 22 At least 40°C below the Bs temperature.
4. The quenching and baining heat treatment method for 165ksi grade oil casing according to any one of claims 1-3, characterized in that, The 165ksi grade carbide-free bainitic / martensitic composite microstructure is used to manufacture oil casing, and the yield strength R of the oil casing is... p0.2 ≥1180MPa, tensile strength R m ≥1350MPa, elongation after fracture A≥16%, transverse impact energy (0℃) A kv ≥100J.
Citation Information
Patent Citations
Low alloy steel for producing 170ksi steel-grade steel pipe
CN107916366A
A high-strength niobium-containing oil casing based on controlled cooling and its preparation method
CN114196885B
A 160 ksi grade high strength and toughness non-standard oil casing and a production method thereof
CN116657045B
Preparation method of P110-grade expansion tube for exploiting petroleum and gas
CN102534372A
Method for preparing 1380MPa grade bainite steel rail by waste heat quenching-self partition
CN110592354A