Design method of impregnation solution for increasing amine loading on activated carbon

By calculating the intersection area between the impregnation solution and the pore size distribution of activated carbon, suitable impregnation solution components were selected and loaded amine-based activated carbon was prepared. This solved the problem of insufficient selectivity of activated carbon in adsorbing formaldehyde, achieving efficient loading and simplified experimentation.

CN117953980BActive Publication Date: 2026-11-20SUN YAT SEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410040943.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-10
Publication Date
2026-11-20
Estimated Expiration
2044-01-10

AI Technical Summary

Technical Problem

In existing technologies, activated carbon lacks selectivity when adsorbing formaldehyde, and the process of selecting a suitable modified solvent and preparing high-loading amine-based activated carbon is complex, resulting in a large workload for experiments.

Method used

By calculating the intersection area of ​​the molecular size distribution function of the impregnation solution and the pore size distribution curve of activated carbon, suitable impregnation solution components can be quickly screened, and activated carbon loaded with amine groups can be prepared by constant temperature water bath shaker reaction.

Benefits of technology

The experiment reduced the time required for solvent selection, improved the adsorption capacity and loading efficiency of activated carbon, simplified the experimental process, obtained a high content of amine loading, and enhanced the adsorption performance of activated carbon.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117953980B_ABST
    Figure CN117953980B_ABST
Patent Text Reader

Abstract

The application discloses a design method of impregnation liquid for increasing amine group loading capacity of activated carbon, and relates to the technical field of activated carbon modification. The design method comprises the following steps: detecting and calculating a distribution function D(r) of molecular size in a liquid phase by using a plurality of impregnation liquids with the same concentration; simulating the pore size distribution of activated carbon by using an NLDFT model to obtain a pore size distribution curve F(w); and calculating the intersection area epsilon of F(w) and D(r) to screen the impregnation liquid with the minimum intersection area epsilon. The design method can reduce the test time consumed by solvent selection, facilitate and expedite the screening of impregnation liquid components suitable for activated carbon pore adsorption, and the activated carbon prepared by using the screened impregnation liquid has strong adsorption capacity and high loading efficiency, can realize high content loading of amine groups, and reduces the workload of screening adsorbates in experiments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of activated carbon modification technology, and in particular to a design method for an impregnation solution to increase the amine loading of activated carbon. Background Technology

[0002] Formaldehyde levels slightly above standard can cause chronic poisoning and are a globally recognized carcinogen, posing significant harm to the human nervous and respiratory systems. When indoor formaldehyde concentrations reach a certain level, it can cause respiratory discomfort, nausea, vomiting, and other adverse symptoms. In severe cases, it can damage the lungs and central nervous system, and even cause chromosomal abnormalities. Photocatalytic oxidation, adsorption, and catalytic oxidation are currently hot research topics in formaldehyde removal methods. Among these, adsorption technology, particularly the adsorbent and its mass, has the potential for recycling, making it considered a highly efficient and economical method for removing indoor formaldehyde. Activated carbon, due to its large specific surface area, abundant pore structure, and high adsorption capacity, is widely used for the purification of indoor VOCs.

[0003] However, since the adsorption behavior of activated carbon itself is non-selective, surface modification is usually required to improve its performance. The adsorption capacity of activated carbon for specific target pollutants can be tuned through activation modifications. These modifications include changes in porosity, surface chemistry, or functional groups on the activated carbon surface. By introducing specific surface modifications, the selectivity of activated carbon can be improved, thereby removing target substances more effectively. Various surface modification methods exist to improve the adsorption performance of activated carbon. For example, amines and formaldehyde can condense to form methyleneimine (carbonyl compound-amine condensation reaction). The imine is protonated by formic acid to generate imine ions, which is important for formaldehyde adsorption. Therefore, the loading of amine groups on the activated carbon surface becomes crucial.

[0004] In the process of using solvents to modify the surface of activated carbon to achieve amine-loaded adsorption, it is necessary to screen solvent molecules suitable for the pore size distribution of activated carbon. This can reduce the workload of solvent selection, lower trial-and-error costs, and ultimately prepare activated carbon with highly loaded amine groups. Therefore, how to obtain suitable modification solvents and how to prepare suitable loaded activated carbon have become key research issues. Summary of the Invention

[0005] This invention provides a design method for impregnating solutions to improve the amine loading of activated carbon, thereby rapidly screening impregnating solution components suitable for the pore size of activated carbon, reducing the workload of adsorbate screening in experiments, and preparing solutions with strong adsorption capacity and high loading efficiency.

[0006] To address the aforementioned technical problems, one objective of this invention is to provide a method for designing an impregnation solution to increase the amine loading of activated carbon, comprising the following steps:

[0007] (1) The molecular size distribution function D(r) in the liquid phase was obtained by detecting and calculating multiple impregnation solutions of the same concentration;

[0008] (2) Select activated carbon and use the NLDFT model to simulate the pore size distribution of activated carbon to obtain the pore size distribution curve F(w) with the pore volume as the vertical axis.

[0009] (3) Integrate the pore size distribution curve F(w) of activated carbon and the distribution function D(r) of the impregnation solution onto a single graph, calculate the intersection area ε between the two, and obtain the impregnation solution for increasing the amine loading of activated carbon by screening the impregnation solution with the smallest intersection area ε.

[0010] As a preferred embodiment, in step (1), the impregnation solution is at least one of diethylenetriamine, triethylenetetramine, tetraethylenepentamine, N,N-dimethylformamide, hexamethyleneimine, p-nitroaniline, and azobisisobutyronitrile.

[0011] As a preferred embodiment, in step (2), the activated carbon is selected to have an average pore size of less than 5 nm and an average micropore volume of greater than 0.03 cm³. 3 / g.

[0012] The average pore size of the activated carbon is less than 5 nm, indicating that it is mainly composed of micropores and some small mesopores. Micropores are the main contributor to the adsorption performance of activated carbon, while mesopores also have a certain influence on the adsorption properties of activated carbon. The average micropore volume is greater than 0.03 cm³. 3 The / g indicates that the activated carbon has a large number of micropores and a large total pore volume, which can improve the adsorption capacity.

[0013] As a preferred embodiment, in step (1), the formula for calculating the molecular size distribution function D(r) in the liquid phase is: Where r is the molecular dynamic radius, μ is the average molecular dynamic radius, and σ is the standard deviation;

[0014] Meanwhile, the formula for calculating the molecular dynamic radius r is as follows: r = kT / (6πnx); where r is the molecular dynamic radius; k is the Boltzmann constant; T is the temperature; η is the viscosity of the dissolving medium; and x is the dynamic radius of the solute molecule.

[0015] As a preferred option, in step (1), for impregnation solutions with multiple components, the pore size distribution data of the molecular size distribution function D(r) of different components in the liquid phase are merged into a large dataset, and the mean and standard deviation of the merged dataset are calculated as the initial values ​​for fitting the normal distribution. The mean and standard deviation of the normal distribution are fitted using the least squares method to obtain the optimal fitting parameters D(r').

[0016] As a preferred embodiment, in step (2), the formula for calculating the activated carbon pore size distribution curve F(w) is: Where N(P / P0) represents the adsorption isotherm data of activated carbon, and w max w is the maximum aperture value. min Let W(P / P0, w) be the minimum pore size, W(P / P0, w) be the adsorption isotherm of a single pore with a pore width of w, and F(w) be the pore size distribution function.

[0017] As a preferred embodiment, in step (3), the formula for calculating the intersection area ε of the distribution function D(r) of the impregnation solution and the pore size distribution curve F(w) of the activated carbon is:

[0018] To address the aforementioned technical problems, a second objective of this invention is to provide a method for preparing amine-loaded activated carbon, comprising the following steps:

[0019] After drying, the activated carbon is mixed with an impregnation solution containing 5-15 wt% solvent in a sealed container and reacted in a constant temperature water bath shaker at 293-333 K. After filtration, the activated carbon is dried to obtain amine-loaded activated carbon.

[0020] The solvent is tetraethylenepentamine or a mixture thereof, wherein the mixture is tetraethylenepentamine and diethylenetriamine.

[0021] As a preferred embodiment, the activated carbon has an average pore size of less than 5 nm and an average micropore volume of greater than 0.03 cm³. 3 / g, activated carbon with a specific surface area greater than 1000 cm² 2 / g.

[0022] As a preferred embodiment, the activated carbon is selected from at least one of coconut shell activated carbon, apricot shell activated carbon, walnut shell activated carbon, wood activated carbon, coal-derived activated carbon, rice husk activated carbon, and regenerated activated carbon.

[0023] As a preferred embodiment, the mixture is tetraethylenepentamine and diethylenetriamine in a mass ratio of 1:1.

[0024] As a preferred embodiment, the mass ratio of activated carbon to impregnation solution is 1:(6-8).

[0025] As a preferred option, the speed of the constant temperature water bath shaker is 120 r / min, and the reaction time is more than 2 hours.

[0026] As a preferred method, the drying temperature is 60-100℃ and the drying time is 24-48 hours.

[0027] To address the aforementioned technical problems, a third objective of this invention is to provide an activated carbon loaded with amine groups.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] The design method employed in this invention can reduce the experimental time spent on solvent selection. The optimal impregnation liquid composition for activated carbon is determined by the intersection area ε of the distribution function D(r) of the impregnation liquid and the pore size distribution curve F(w) of the activated carbon. This allows for convenient and rapid screening of impregnation liquid components suitable for the pore size adsorption of activated carbon. Activated carbon prepared from the impregnation liquid obtained by the method of this invention has strong adsorption capacity and high loading efficiency, and can achieve high content loading of amine groups, reducing the workload of adsorbate screening in experiments. Attached Figure Description

[0030] Figure 1 : The distribution function curve D(r1) of the TEPA solution and the pore size distribution curve F(w) of the activated carbon in Example 1 of the present invention (Note: The gray part is the pore size intersection area ε);

[0031] Figure 2 : The distribution function curve D(r2) of the DETA solution and the pore size distribution curve F(w) of the activated carbon in Example 1 of the present invention (Note: The gray part is the pore size intersection area ε);

[0032] Figure 3 : This represents the distribution function curve D(r3) of the TEPA and DETA mixed solution and the pore size distribution curve F(w) of activated carbon in Example 1 of this invention (Note: The gray part is the pore size intersection area ε). Detailed Implementation

[0033] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0034] The activated carbon, TEPA (tetraethylenepentamine), DETA (diethylenetriamine), and TETA (triethylenetetraamine) used in Examples 1-5 below all have the same source and characteristic parameters.

[0035] Example 1

[0036] A method for designing an impregnation solution to increase the amine loading of activated carbon includes the following steps:

[0037] (1) For single-component impregnation solutions such as TEPA or DETA, the molecular dynamic radii r of TEPA and DETA are substituted into Formula 2) to calculate the molecular size distribution functions D(r1) and D(r2) of the 10wt% impregnation solution in the liquid phase. The average molecular size μ of TEPA is 0.6079 and the standard deviation α is 0.3. The average molecular size μ of DETA is 0.5138 and the standard deviation α is 0.3.

[0038] Equation 1) The formula for calculating the molecular dynamic radius r is as follows:

[0039] r = kT / (6πnx);

[0040] Where r is the molecular dynamic radius; k is the Boltzmann constant; T is the temperature; η is the viscosity of the dissolving medium; and x is the dynamic radius of the solute molecule.

[0041] The formula for calculating the distribution function D(r) in Equation 2) is as follows:

[0042]

[0043] Where r is the molecular dynamic radius, μ is the average molecular dynamic radius, and σ is the standard deviation;

[0044] (2) For impregnation solutions with multiple components, such as a mixture of TEPA and DETA with a mass ratio of 1:1, the pore size distribution data of the distribution functions D(r1) and D(r2) of TEPA and DETA are merged into a large dataset. The mean and standard deviation of the merged dataset are calculated as the initial values ​​for fitting the normal distribution. The average value μ of the molecular size is 0.5535 and the standard deviation σ is 0.3981. The mean and standard deviation of the normal distribution are fitted using the least squares method to obtain the optimal fitting parameter D(r3).

[0045] (3) Coconut shell activated carbon with an average pore size of less than 5 nm and an average micropore volume greater than 0.03 cm³ was selected. 3 / g, activated carbon with a specific surface area greater than 1000 cm² 2 / g, the pore size distribution of activated carbon was simulated using the NLDFT model, and the pore size distribution curve F(w) with pore volume as the ordinate was obtained. This curve was plotted with D(r) on the same graph, and the intersection area ε between the two curves was calculated according to formula 4). Where, as Figure 1 As shown, the area of ​​intersection between the pore sizes of TEPA and activated carbon is ε = 0.45248. Figure 2 As shown, the area of ​​intersection between DETA and activated carbon pore size is ε = 1.30565, as... Figure 3 As shown, the area of ​​intersection between the TEPA and DETA mixture and the activated carbon pore size is ε = 0.87671.

[0046] Herein, the calculation method for the pore size distribution of activated carbon is shown in the following Formula 3):

[0047]

[0048] Herein, N(P / P0) is the experimental adsorption isotherm data of activated carbon, w max is the maximum pore size, w min is the minimum pore size, W(P / P0, w) is the adsorption isotherm of a single pore with a pore width of w, F(w) is the pore size distribution function, F(w) is a function obtained from the formula W(P / P0, w), and is the set of all W(P / P0, w); the NLDFT equation is used to describe the pore size distribution on the surface of activated carbon, the (GAI) equation can be obtained from the adsorption isotherm measured by a microscopic method and the experimental isotherm measured on a porous solid, a set of N(P / P0, W) isotherms can be obtained by DFT or MC simulation given the adsorbate / adsorbent, and the pore size distribution curve F(w) can be derived by solving the GAI equation through the fast non-negative least squares method;

[0049] (4) Draw the pore size distribution curve F(w) of activated carbon and the distribution function D(r) of the impregnation solution on the same graph, and calculate the intersection area ε of the two according to Formula 4), wherein, as Figure 1 shown, the intersection area ε between TEPA and the pore size of activated carbon is 0.45248, as Figure 2 shown, the intersection area ε between DETA and the pore size of activated carbon is 1.30565, as Figure 3 shown, the intersection area ε between the mixed solution of TEPA and DETA and the pore size of activated carbon is 0.87671. The smaller the intersection area ε, the larger the loading capacity of the impregnation solution on the activated carbon, wherein the TEPA solution < the mixed solution of TEPA and DETA < the DETA solution. By screening the impregnation solution with the smallest intersection area ε, the impregnation solution that can increase the amine-based loading capacity of activated carbon can be obtained;

[0050] Herein, the calculation of the intersection area between the molecular size D(r) of the impregnation solution and the pore size distribution F(w) of activated carbon is shown in the following Formula 4):

[0051]

[0052] Embodiment 2

[0053] A preparation method of amine-loaded activated carbon comprises the following steps:

[0054] The activated carbon with an average pore size less than 5 nm and an average micropore volume greater than 0.03 cm 3 / g and a specific surface area greater than 1000 cm 2 / g of coconut shell activated carbon was dried in a vacuum drying oven at 80℃ for 24 hours. A 10% TEPA aqueous solution was selected as the impregnation solution. 5g of activated carbon and 30g of TEPA solution were mixed in a sealed glass reagent bottle. The reagent bottle was placed in a constant temperature water bath shaker and shaken at 120r / min at 303K for 24 hours. The solution was separated by filtration. The activated carbon was then dried in an oven to prepare TEPA-loaded activated carbon L-1.

[0055] Example 3

[0056] A method for preparing amine-loaded activated carbon includes the following steps:

[0057] The average pore size is less than 5 nm and the average micropore volume is greater than 0.03 cm³. 3 / g, specific surface area greater than 1000cm³ 2 / g of coconut shell activated carbon was dried in a vacuum drying oven at 80℃ for 24 hours. A 10% mass concentration DETA aqueous solution was selected as the impregnation solution. 5g of activated carbon and 30g of DETA solution were mixed in a sealed glass reagent bottle. The reagent bottle was placed in a constant temperature water bath shaker and shaken at 120r / min at 303K for 24 hours. The solution was separated by filtration. The activated carbon was then dried in an oven to prepare DETA-loaded activated carbon L-2.

[0058] Example 4

[0059] A method for preparing amine-loaded activated carbon includes the following steps:

[0060] The average pore size is less than 5 nm and the average micropore volume is greater than 0.03 cm³. 3 / g, specific surface area greater than 1000cm³ 2 / g of coconut shell activated carbon was dried in a vacuum drying oven at 80℃ for 24 hours. A 1:1 mass ratio of TEPA and DETA aqueous solution was selected as the impregnation solution with a mass concentration of 10%. 5g of activated carbon and 30g of the mixed solution were mixed in a sealed glass reagent bottle. The reagent bottle was placed in a constant temperature water bath shaker and shaken at 120r / min at 303K for 24 hours. The solution was separated by filtration, and the activated carbon was dried in an oven to prepare activated carbon L-3 loaded with TEPA and DETA.

[0061] Example 5

[0062] A method for preparing amine-loaded activated carbon includes the following steps:

[0063] The average pore size is less than 5 nm and the average micropore volume is greater than 0.03 cm³. 3 / g, specific surface area greater than 1000cm³2 / g of coconut shell activated carbon was dried in a vacuum drying oven at 80℃ for 24 hours. TETA aqueous solution with a mass concentration of 10% was selected as the impregnation solution. 5g of activated carbon and 30g of TETA solution were mixed in a sealed glass reagent bottle. The reagent bottle was placed in a constant temperature water bath shaker and shaken at 120r / min at 303K for 24 hours. The solution was separated by filtration, and the activated carbon was dried in an oven to prepare TETA-loaded activated carbon L-4.

[0064] Performance testing

[0065] The above-prepared supported activated carbons L-1, L-2, L-3, and L-4 were subjected to equilibrium adsorption capacity q. e The concentration of the impregnation solution loaded on the activated carbon was determined by the (mg / g) test. The results are shown in Table 1 below and can be calculated using the following equation:

[0066]

[0067] Among them, C0 (mg / L) and C e (mg / L) represent the initial and equilibrium concentrations of the impregnation solution, respectively; V(L) is the solution volume; and M(g) is the mass of activated carbon.

[0068] Table 1 - Results of the loading of impregnation solution on the activated carbon surface in Examples 2-5 of this application

[0069]

[0070] Based on the experimental results, it can be observed that the order of impregnation solution loading in Examples 2-5 is TEPA > MIX > TETA > DETA, which is consistent with... Figure 1-3 The area of ​​the size distribution function ε matches, verifying the effectiveness of the impregnation solution used to improve the screening of amine-loaded activated carbon in this invention, and supporting the feasibility of the design method of this invention. Experimental data show that the activated carbon with higher amine loading prepared by the impregnation solution obtained by the method of this invention has strong adsorption capacity and high loading efficiency, reducing the workload of adsorbate screening in experiments.

[0071] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above descriptions are merely specific embodiments of the present invention and are not intended to limit the scope of protection of the present invention. In particular, it should be noted that any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention for those skilled in the art.

Claims

1. A method for designing an impregnation solution to increase the amine loading of activated carbon, characterized in that, Includes the following steps: (1) Detect and calculate the molecular size distribution function D(r) in the liquid phase by using multiple impregnation solutions of the same concentration; (2) Select activated carbon and use the NLDFT model to simulate the pore size distribution of activated carbon to obtain the pore size distribution curve F(w) with the pore volume as the vertical axis; (3) Integrate the pore size distribution curve F(w) of activated carbon and the distribution function D(r) of impregnation solution onto a single graph and calculate the area of ​​intersection between the two. By screening the intersection area The smallest amount of impregnation solution is needed to obtain an impregnation solution that can increase the amine loading of activated carbon; In step (1), the impregnation solution is at least one of diethylenetriamine, triethylenetetramine, tetraethylenepentamine, N,N-dimethylformamide, hexamethyleneimine, p-nitroaniline, and azobisisobutyronitrile; In step (2), the activated carbon is selected to have an average pore size of less than 5 nm and an average micropore volume of greater than 0.03 cm³. 3 / g.

2. The design method of an impregnation solution for increasing the amine loading of activated carbon as described in claim 1, characterized in that, In step (1), the formula for calculating the molecular size distribution function D(r) in the liquid phase is: Where r is the molecular dynamic radius, μ is the average molecular dynamic radius, and σ is the standard deviation; Meanwhile, the formula for calculating the molecular dynamic radius r is as follows: ; Where r is the molecular dynamic radius; k is the Boltzmann constant; T is the temperature; η is the viscosity of the dissolving medium; and x is the dynamic radius of the solute molecule.

3. The design method of an impregnation solution for increasing the amine loading of activated carbon as described in claim 2, characterized in that, In step (1), for impregnation solutions with multiple components, the pore size distribution data of the molecular size distribution function D(r) of different components in the liquid phase are merged into a large dataset. The mean and standard deviation of the merged dataset are calculated as the initial values ​​for fitting the normal distribution. The mean and standard deviation of the normal distribution are fitted using the least squares method to obtain the optimal fitting parameters D(r').

4. The design method of an impregnation solution for increasing the amine loading of activated carbon as described in claim 1, characterized in that, In step (2), the formula for calculating the activated carbon pore size distribution curve F(w) is: Where N(P / P0) represents the adsorption isotherm data of activated carbon, and w max w is the maximum aperture value. min Let W(P / P0, w) be the minimum pore size, W(P / P0, w) be the adsorption isotherm of a single pore with a pore width of w, and F(w) be the pore size distribution function.

5. The design method of an impregnation solution for increasing the amine loading of activated carbon as described in claim 1, characterized in that, In step (3), the area of ​​intersection between the distribution function D(r) of the impregnation solution and the pore size distribution curve F(w) of the activated carbon is... The calculation formula is: .

6. The design method of an impregnation solution for increasing the amine loading of activated carbon as described in claim 1, characterized in that, The activated carbon has an average pore size of less than 5 nm and an average micropore volume of greater than 0.03 cm³. 3 / g, activated carbon with a specific surface area greater than 1000 cm² 2 / g; The activated carbon is selected from at least one of coconut shell activated carbon, apricot shell activated carbon, walnut shell activated carbon, wood activated carbon, coal-derived activated carbon, rice husk activated carbon, and regenerated activated carbon.