Light emitting diode epitaxial wafer and preparation method thereof, and light emitting diode

By introducing a hole injection structure consisting of a Si₃N₄ layer and a P-type AlGaN/InN superlattice layer into the epitaxial wafer of a light-emitting diode, the problems of low hole concentration and migration rate are solved, achieving efficient hole injection and improved luminous efficiency.

CN117954539BActive Publication Date: 2026-11-24JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410055366.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-15
Publication Date
2026-11-24
Estimated Expiration
2044-01-15

Smart Images

  • Figure CN117954539B_ABST
    Figure CN117954539B_ABST
Patent Text Reader

Abstract

This invention discloses a light-emitting diode (LED) epitaxial wafer and its fabrication method, as well as the LED itself. The LED epitaxial wafer includes a substrate and a buffer layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, a hole injection layer, an electron blocking layer, and a P-type GaN layer sequentially stacked on the substrate. The hole injection layer includes a Si3N4 layer, a P-type AlGaN / InN superlattice layer, and a P-type InGaN layer sequentially stacked on the multiple quantum well layer. The P-type AlGaN / InN superlattice layer comprises periodically alternating layers of P-type AlGaN and InN layers. The hole injection layer of this invention can improve the hole concentration and injection efficiency, and increase the radiative recombination efficiency of electrons and holes in the multiple quantum well layer, thereby improving the luminous efficiency of the LED.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor technology, and in particular to a light-emitting diode epitaxial wafer and its fabrication method, and a light-emitting diode. Background Technology

[0002] In light-emitting diodes (LEDs), because the concentration and migration rate of holes are much lower than those of electrons, the hole concentration injected into the multi-quantum-well (MFU) emitting region is much lower than the electron concentration. Holes are mainly concentrated in a few quantum wells near the P-type layer, resulting in a small number of quantum wells that actually emit light. Furthermore, electrons can easily cross the active region into the P-type layer, causing electron leakage and affecting the performance of the LED. Therefore, it is necessary to increase the doping concentration of the P-type layer to increase the hole concentration injected into the MFU emitting region. However, the Mg acceptor in P-type GaN has a deep energy level of approximately 170 meV, and the ionization rate of Mg at room temperature is only about 1%. In addition, the MOCVD method for growing Mg-doped P-type GaN introduces a large amount of H atoms, which passivate the Mg acceptors, significantly increasing the activation energy of the Mg acceptors. Therefore, it is difficult to obtain P-type GaN materials with high hole concentrations. Summary of the Invention

[0003] The technical problem to be solved by the present invention is to provide an epitaxial wafer for a light-emitting diode that can improve hole injection efficiency, thereby improving luminous efficiency.

[0004] The technical problem to be solved by the present invention is to provide a method for preparing an epitaxial wafer of a light-emitting diode, which is simple in process and produces an epitaxial wafer of a light-emitting diode with high luminous efficiency.

[0005] To achieve the above-mentioned technical effects, the present invention provides a light-emitting diode epitaxial wafer, comprising a substrate and a buffer layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, a hole injection layer, an electron blocking layer, and a P-type GaN layer sequentially stacked on the substrate. The hole injection layer comprises a Si3N4 layer, a P-type AlGaN / InN superlattice layer, and a P-type InGaN layer sequentially stacked on the multiple quantum well layer. The P-type AlGaN / InN superlattice layer comprises periodically alternating layers of P-type AlGaN layers and InN layers.

[0006] As an improvement to the above technical solution, the thickness of the Si3N4 layer is 1nm to 10nm.

[0007] As an improvement to the above technical solution, the growth period of the P-type AlGaN / InN superlattice layer is 1–20, the thickness of the P-type AlGaN layer is 1 nm–50 nm, the Al composition ratio is 0.01–0.5, and the Mg doping concentration is 1 × 10⁻⁶. 18 cm -3 ~1×1020 cm -3 The thickness of the InN layer is 0.5 nm to 5 nm.

[0008] As an improvement to the above technical solution, the thickness of the p-type InGaN layer is 5nm to 100nm, the In composition ratio is 0.01 to 0.3%, and the Mg doping concentration is 1×10⁻⁶. 19 cm -3 ~1×10 21 cm -3 .

[0009] As an improvement to the above technical solution, the electron blocking layer is an AlInGaN layer with a thickness of 10nm to 40nm, an Al composition ratio of 0.01 to 0.1%, and an In composition ratio of 0.01 to 0.2%.

[0010] Accordingly, the present invention also discloses a method for preparing a light-emitting diode epitaxial wafer, which includes the following steps:

[0011] A substrate is provided on which a buffer layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, a hole injection layer, an electron blocking layer, and a P-type GaN layer are sequentially grown. The hole injection layer comprises a Si3N4 layer, a P-type AlGaN / InN superlattice layer, and a P-type InGaN layer sequentially stacked on the multiple quantum well layer. The P-type AlGaN / InN superlattice layer comprises periodically alternating layers of P-type AlGaN and InN layers.

[0012] As an improvement to the above technical solution, the growth temperature of the Si3N4 layer is 800℃~900℃, and the growth pressure is 50Torr~500Torr.

[0013] As an improvement to the above technical solution, the growth temperature of the P-type AlGaN layer is 650℃~800℃, and the growth pressure is 50Torr~500Torr.

[0014] The growth temperature of the InN layer is 650℃~800℃, and the growth pressure is 50Torr~500Torr.

[0015] As an improvement to the above technical solution, the growth temperature of the P-type InGaN layer is 650℃~800℃, and the growth pressure is 50Torr~500Torr.

[0016] Accordingly, the present invention also discloses a light-emitting diode, including the above-mentioned light-emitting diode epitaxial wafer.

[0017] Implementing the embodiments of the present invention has the following beneficial effects:

[0018] The hole injection layer of the present invention comprises a Si3N4 layer, a P-type AlGaN / InN superlattice layer and a P-type InGaN layer stacked sequentially, which can improve the hole concentration and hole injection efficiency of the P-type layer, thereby improving the radiative recombination efficiency of electrons and holes in the multi-quantum well layer; blocking the extension of defects and reducing the electron overflow effect, thereby reducing the leakage current of the light-emitting diode and improving the luminous efficiency of the light-emitting diode. The deposition of Si3N4 layers can reduce the extension of V-shaped pit defects, improve the quality of subsequent crystal growth, reduce leakage current in LEDs, and improve aging performance. The high potential barrier of the P-type AlGaN layer can reduce non-radiative recombination caused by electron overflow from the multi-quantum well layer to the P-type GaN layer, while improving the efficiency of hole injection into the multi-quantum well layer. The narrow bandgap of the InN layer forms a potential well layer to store holes. The superlattice structure composed of P-type AlGaN / InN layers can promote more uniform hole injection into the multi-quantum well layer and improve the radiative recombination efficiency of electrons and holes. The P-type InGaN layer reduces the activation energy of Mg by doping In and increases the concentration of activated Mg, providing sufficient holes and electrons for recombination in the LED and improving the luminous efficiency of the LED. Attached Figure Description

[0019] Figure 1 This is a schematic diagram of the structure of the light-emitting diode epitaxial wafer provided in an embodiment of the present invention;

[0020] Figure 2 This is a schematic diagram of the hole injection layer of the light-emitting diode epitaxial wafer provided in an embodiment of the present invention;

[0021] Figure 3 This is a flowchart of the method for fabricating a light-emitting diode epitaxial wafer provided in an embodiment of the present invention. Detailed Implementation

[0022] To make the objectives, technical solutions, and advantages of the present invention clearer, the present invention will be further described in detail below with reference to specific embodiments.

[0023] like Figure 1As shown, this embodiment of the invention provides a light-emitting diode epitaxial wafer, including a substrate 1 and a buffer layer 2, an undoped GaN layer 3, an N-type GaN layer 4, a multiple quantum well layer 5, a hole injection layer 6, an electron blocking layer 7, and a P-type GaN layer 8 sequentially stacked on the substrate 1. The hole injection layer 6 includes a Si3N4 layer 61, a P-type AlGaN / InN superlattice layer 62, and a P-type InGaN layer 63 sequentially stacked on the multiple quantum well layer 5; the P-type AlGaN / InN superlattice layer 62 includes periodically alternating P-type AlGaN layers 621 and InN layers 622. The hole injection layer 6 of this invention can improve the luminous efficiency of the light-emitting diode. On the one hand, it increases the hole concentration and hole injection efficiency of the P-type layer, thereby improving the radiative recombination efficiency of electrons and holes in the multiple quantum well layer; on the other hand, it blocks the extension of defects, reduces the electron overflow effect, and thus reduces the leakage current of the light-emitting diode.

[0024] In one embodiment, the thickness of the Si3N4 layer is 1 nm to 10 nm. If the thickness is less than 1 nm, it cannot effectively block defects; if the thickness is greater than 10 nm, it will lead to increased lattice mismatch, resulting in a decrease in the crystal quality of the subsequently deposited epitaxial layer. Examples of thicknesses are 1 nm, 3 nm, 5 nm, 7 nm, 9 nm, or 10 nm, but are not limited to these. Depositing the Si3N4 layer can reduce the extension of V-type pit defects into the P-type layer, improve the crystal quality of the P-type layer, reduce leakage current in the light-emitting diode, and improve aging performance.

[0025] In one embodiment, the growth cycle of the P-type AlGaN / InN superlattice layer is 1 to 20. The thickness of the P-type AlGaN layer is 1 nm to 50 nm. If the thickness is less than 1 nm, it cannot effectively block electron overflow; if the thickness is greater than 50 nm, it will result in an excessively high potential barrier. Examples of thicknesses are 1 nm, 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, or 50 nm, but not limited to these. The Al content of the P-type AlGaN layer is 0.01 to 0.5. An excessively high Al content will result in a low Mg activation rate and a decrease in crystal quality. Examples of Al content are 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, or 0.5, but not limited to these. The Mg doping concentration of the P-type AlGaN layer is 1 × 10⁻⁶. 18 cm -3 ~1×10 20 cm -3 If the Mg doping concentration is too low, it will hinder hole injection; if the Mg doping concentration is too high, it will cause a decrease in crystal quality. An example is 1×10⁻⁶. 18 cm -3 5×10 18 cm -3 8×10 18 cm-3 1×10 19 cm -3 5×10 19 cm -3 Or 1×10 20 cm -3 However, this is not the only consideration. The thickness of the InN layer is 0.5 nm to 5 nm. Excessive thickness will cause a decrease in crystal quality. Examples of thicknesses are 0.5 nm, 0.8 nm, 1 nm, 2 nm, 3.5 nm, or 5 nm, but this is not the only consideration. The high potential barrier of the P-type AlGaN layer can reduce the nonradiative recombination caused by electrons overflowing from the multi-quantum well layer to the P-type layer. A small amount of Mg doping can improve the efficiency of hole injection into the multi-quantum well layer. The narrow bandgap of the InN layer forms a potential well layer to store holes. The superlattice structure of alternating layers of the two forms a potential well / barrier structure, which can promote more uniform hole injection into the multi-quantum well layer, improve the radiative recombination efficiency of electrons and holes, and improve the uniformity of light emission.

[0026] In one embodiment, the thickness of the P-type InGaN layer is 5 nm to 100 nm, exemplarily 5 nm, 10 nm, 20 nm, 40 nm, 60 nm, 80 nm, or 100 nm, but not limited thereto. The In composition ratio of the P-type InGaN layer is 0.01 to 0.3, exemplarily 0.01, 0.03, 0.05, 0.08, 0.1, 0.2, or 0.3, but not limited thereto. The Mg doping concentration of the P-type InGaN layer is 1 × 10⁻⁶. 19 cm -3 ~1×10 21 cm -3 An example is 1×10 19 cm -3 5×10 19 cm -3 8×10 19 cm -3 1×10 20 cm -3 5×10 20 cm -3 Or 1×10 21 cm -3 However, this is not the only benefit. Doping with In can lower the activation energy of Mg and increase the concentration of activated Mg, thereby increasing the hole concentration. This provides sufficient holes for recombination with electrons in the LED, thus improving the luminous efficiency of the LED.

[0027] In one embodiment, the electron blocking layer is an AlInGaN layer with a thickness of 10nm to 40nm, exemplarily 10nm, 15nm, 20nm, 25nm, 30nm, or 40nm, but not limited thereto. The Al composition of the electron blocking layer is 0.01 to 0.1%, exemplarily 0.01, 0.03, 0.05, 0.08, or 0.1, but not limited thereto. The In composition of the electron blocking layer is 0.01 to 0.2%, exemplarily 0.01, 0.03, 0.05, 0.08, 0.1, or 0.2, but not limited thereto. Since the hole injection layer partially blocks electrons, the thickness of the electron blocking layer can be appropriately reduced.

[0028] In addition to the hole injection layer and electron blocking layer structures described above, the other layered structures of the present invention have the following characteristics:

[0029] The substrate 1 can be selected from one of the following: sapphire substrate, SiO2 sapphire composite substrate, silicon substrate, silicon carbide substrate, gallium nitride substrate, and zinc oxide substrate. Specifically, the substrate 1 is selected as a sapphire substrate. Sapphire is currently the most commonly used GaN-based LED substrate material. Sapphire substrates have mature manufacturing processes, low prices, are easy to clean and process, and have good stability at high temperatures.

[0030] The buffer layer 2 is an AlN buffer layer or an AlGaN buffer layer. In one embodiment, the buffer layer 2 is an AlN buffer layer with a thickness of 10nm to 50nm. The AlN buffer layer provides nucleation centers with the same orientation as the substrate, releasing the stress caused by the lattice mismatch between GaN and the substrate, as well as the thermal stress caused by the mismatch in the coefficient of thermal expansion. This provides a flat nucleation surface for subsequent growth, reduces the contact angle of nucleation growth, and enables the island-shaped GaN grains to connect into a surface within a smaller thickness, transforming into two-dimensional epitaxial growth.

[0031] The thickness of the undoped GaN layer 3 is 1 μm to 5 μm.

[0032] The thickness of the N-type GaN layer 4 is 2μm to 3μm, and the Si doping concentration is 1×10⁻⁶. 19 cm -3 ~5×10 19 cm -3 .

[0033] The multi-quantum-well light-emitting layer 5 comprises periodically stacked InGaN quantum well layers and AlGaN quantum barrier layers, with a stacking period of 6 to 12. The InGaN quantum well layer has a thickness of 2 nm to 5 nm and an In composition ratio of 0.1 to 0.3; the AlGaN quantum barrier layer has a thickness of 5 nm to 15 nm and an Al composition ratio of 0.01 to 0.1.

[0034] The thickness of the p-type GaN layer 8 is 10 nm to 50 nm, and the Mg doping concentration is 1 × 10⁸. 19 cm -3 ~1×10 21 cm -3 .

[0035] Correspondingly, such as Figure 2 As shown, the present invention also provides a method for fabricating a light-emitting diode epitaxial wafer, comprising the following steps:

[0036] S1. Provide a substrate;

[0037] The substrate can be one of sapphire substrate, SiO2 sapphire composite substrate, silicon substrate, silicon carbide substrate, gallium nitride substrate, and zinc oxide substrate. In one embodiment, a sapphire substrate is selected as the substrate. Nitriding treatment is performed in an NH3 atmosphere for 2 to 20 seconds at a temperature of 800°C to 1100°C.

[0038] S2. A buffer layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, a hole injection layer, an electron blocking layer, and a P-type GaN layer are sequentially grown on the substrate. The epitaxial structure can be grown by MOCVD, MBE, or VPE, but is not limited to these methods. Specifically, S2 includes the following steps:

[0039] S21, growth buffer layer;

[0040] The buffer layer can be either an AlN buffer layer or an AlGaN buffer layer. In one embodiment, the AlN buffer layer is grown using PVD. The sapphire substrate with the AlN buffer layer deposited is transferred into MOCVD and pretreated in an H2 atmosphere for 1 to 10 minutes at a temperature of 1000°C to 1200°C. This pretreatment improves the crystal quality of the AlN buffer layer and can effectively enhance the crystal quality of the subsequently deposited GaN epitaxial layer.

[0041] S22, grow an undoped GaN layer;

[0042] MOCVD growth was employed, with the reaction chamber temperature controlled at 1050℃~1200℃ and the pressure at 100Torr~600Torr. NH3 was introduced as the N source, and TMGa was introduced as the Ga source.

[0043] S23, grow an N-type GaN layer;

[0044] MOCVD growth was employed, with the reaction chamber temperature controlled at 1050℃~1200℃ and the pressure at 100Torr~600Torr. NH3 was introduced as the N source, TMGa as the Ga source, and SiH4 as the N-type doping source.

[0045] S24, Growth of a multi-quantum-well light-emitting layer;

[0046] MOCVD was used to grow InGaN quantum well layers, with the reaction chamber temperature controlled at 790℃~810℃ and the pressure at 50Torr~300Torr. NH3 was introduced as the N source, TMGa as the Ga source, and TMIn as the In source. AlGaN quantum barrier layers were grown by controlling the reaction chamber temperature at 800℃~900℃ and the pressure at 50Torr~300Torr, with NH3 as the N source, TMGa as the Ga source, and TMAl as the Al source. InGaN quantum well layers and AlGaN quantum barrier layers were then repeatedly stacked and periodically grown.

[0047] S25, Growth Hole Injection Layer; Specifically, S25 includes the following steps:

[0048] S251, grow Si3N4 layer;

[0049] CVD growth was employed, with the reaction chamber temperature controlled at 800℃~900℃ and the pressure at 50Torr~500Torr. NH3 was introduced as the N source, and SiH4 was introduced as the Si source.

[0050] S252, grow a P-type AlGaN / InN superlattice layer;

[0051] MOCVD was used to grow P-type AlGaN layers, with the reaction chamber temperature controlled at 650℃~800℃ and the pressure at 50Torr~500Torr. NH3 was introduced as the N source, TMGa as the Ga source, TMAl as the Al source, and Cp2Mg as the P-type doping source. InN layers were grown by controlling the reaction chamber temperature at 650℃~800℃ and the pressure at 50Torr~500Torr, with NH3 as the N source and TMIn as the In source. P-type AlGaN and InN layers were then repeatedly stacked and periodically grown.

[0052] S253, grow a P-type InGaN layer;

[0053] MOCVD growth was employed, with the reaction chamber temperature controlled at 650℃~800℃ and the pressure at 50Torr~500Torr. NH3 was introduced as the N source, TMGa as the Ga source, TMIn as the In source, and Cp2Mg as the P-type doping source.

[0054] S26, Growth of electron blocking layer;

[0055] MOCVD growth was employed, with the reaction chamber temperature controlled at 900℃~1000℃ and the pressure at 100Torr~300Torr. NH3 was introduced as the N source, TMGa as the Ga source, TMAl as the Al source, and TMIn as the In source.

[0056] S27, grow a P-type GaN layer;

[0057] MOCVD growth was employed, with the reaction chamber temperature controlled at 900℃~1050℃ and the pressure at 100Torr~600Torr. NH3 was introduced as the N source, TMGa as the Ga source, and Cp2Mg as the P-type doping source.

[0058] The present invention will be further illustrated below with specific embodiments.

[0059] Example 1

[0060] This embodiment provides a light-emitting diode epitaxial wafer, including a substrate and a buffer layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, a hole injection layer, an electron blocking layer and a P-type GaN layer sequentially stacked on the substrate.

[0061] The substrate is a sapphire substrate.

[0062] The buffer layer is an AlN buffer layer with a thickness of 15nm.

[0063] The thickness of the undoped GaN layer is 2 μm.

[0064] The thickness of the N-type GaN layer is 2 μm, and the Si doping concentration is 2.5 × 10⁻⁶. 19 cm -3 .

[0065] The multiple quantum well layer consists of alternating layers of InGaN quantum wells and AlGaN quantum barriers, with a period of 10. The InGaN quantum well layer is 3.5 nm thick with an In content of 0.22%; the AlGaN quantum barrier layer is 9.8 nm thick with an Al content of 0.05%.

[0066] The hole injection layer consists of a Si3N4 layer, a P-type AlGaN / InN superlattice layer, and a P-type InGaN layer stacked sequentially. The Si3N4 layer has a thickness of 3.5 nm. The P-type AlGaN / InN superlattice layer has 5 periods, the P-type AlGaN layer has a thickness of 5 nm, an Al composition of 0.1%, and a Mg doping concentration of 3 × 10⁻⁶. 19 cm -3 The InN layer is 1.5 nm thick. The p-type InGaN layer is 30 nm thick, with an In composition of 0.05% and a Mg doping concentration of 5 × 10⁻⁶. 20 cm-3 .

[0067] The electron blocking layer is an AlInGaN layer with a thickness of 15 nm, an Al content of 0.1%, and an In content of 0.05%.

[0068] The thickness of the p-type GaN layer is 15 nm, and the Mg doping concentration is 2 × 10⁻⁶. 20 cm -3 .

[0069] The above-mentioned method for fabricating an epitaxial wafer of a light-emitting diode includes the following steps:

[0070] S1. Provide a substrate;

[0071] The substrate used is sapphire, which is nitrided in an NH3 atmosphere for 10 seconds at a temperature of 900℃.

[0072] S2. A buffer layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, a hole injection layer, an electron blocking layer, and a P-type GaN layer are sequentially grown on the substrate, specifically including the following steps:

[0073] S21, growth buffer layer;

[0074] An AlN buffer layer was grown using PVD. The sapphire substrate with the AlN buffer layer deposited was transferred into an MOCVD chamber and pretreated in an H2 atmosphere for 5 minutes at a temperature of 1100°C.

[0075] S22, grow an undoped GaN layer;

[0076] MOCVD growth was employed, with the reaction chamber temperature controlled at 1100℃ and the pressure at 150 Torr. NH3 was introduced as the N source, and TMGa was introduced as the Ga source.

[0077] S23, grow an N-type GaN layer;

[0078] MOCVD growth was employed, with the reaction chamber temperature controlled at 1120℃ and the pressure at 100 Torr. NH3 was introduced as the N source, TMGa as the Ga source, and SiH4 as the N-type doping source.

[0079] S24, Growth of a multi-quantum-well light-emitting layer;

[0080] MOCVD was used to grow InGaN quantum well layers by controlling the reaction chamber temperature at 795℃ and the pressure at 200 Torr, with NH3 as the N source, TMGa as the Ga source, and TMIn as the In source. AlGaN quantum barrier layers were grown by controlling the reaction chamber temperature at 855℃ and the pressure at 200 Torr, with NH3 as the N source, TMGa as the Ga source, and TMAl as the Al source. InGaN quantum well layers and AlGaN quantum barrier layers were then repeatedly stacked and periodically grown.

[0081] S25, Growth Hole Injection Layer; Specifically, S25 includes the following steps:

[0082] S251, grow Si3N4 layer;

[0083] CVD growth was employed, with the reaction chamber temperature controlled at 850℃ and the pressure at 100 Torr. NH3 was introduced as the N source, and SiH4 was introduced as the Si source.

[0084] S252, grow a P-type AlGaN / InN superlattice layer;

[0085] MOCVD was used to grow a P-type AlGaN layer, with the reaction chamber temperature controlled at 700℃ and the pressure at 300 Torr. NH3 was introduced as the N source, TMGa as the Ga source, TMAl as the Al source, and Cp2Mg as the P-type doping source. The reaction chamber temperature was controlled at 700℃ and the pressure at 300 Torr. NH3 was introduced as the N source, and TMIn as the In source, to grow an InN layer. The P-type AlGaN and InN layers were then repeatedly stacked and periodically grown.

[0086] S253, grow a P-type InGaN layer;

[0087] MOCVD growth was employed, with the reaction chamber temperature controlled at 700℃ and the pressure at 300 Torr. NH3 was introduced as the N source, TMGa as the Ga source, TMIn as the In source, and Cp2Mg as the P-type doping source.

[0088] S26, Growth of electron blocking layer;

[0089] MOCVD growth was employed, with the reaction chamber temperature controlled at 965℃ and the pressure at 200 Torr. NH3 was introduced as the N source, TMGa as the Ga source, TMAl as the Al source, and TMIn as the In source.

[0090] S27, grow a P-type GaN layer;

[0091] MOCVD growth was employed, with the reaction chamber temperature controlled at 985℃ and the pressure at 200 Torr. NH3 was introduced as the N source, TMGa as the Ga source, and Cp2Mg as the P-type doping source.

[0092] Example 2

[0093] This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 1 in that the thickness of the Si3N4 layer is 1 nm. All other aspects are the same as in Embodiment 1.

[0094] Example 3

[0095] This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 1 in that the number of periods in the P-type AlGaN / InN superlattice layer is 10, the thickness of the P-type AlGaN layer is 2.5 nm, the Al composition ratio is 0.08, and the Mg doping concentration is 8 × 10⁻⁶. 18 cm -3 The InN layer has a thickness of 1.0 nm. Everything else is the same as in Example 1.

[0096] Example 4

[0097] This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 1 in that the thickness of the P-type InGaN layer is 10 nm, the In composition ratio is 0.1%, and the Mg doping concentration is 8 × 10⁻⁶. 19 cm -3 Everything else is the same as in Example 1.

[0098] Comparative Example 1

[0099] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the hole injection layer does not include a Si3N4 layer; correspondingly, the fabrication method also does not include the Si3N4 layer fabrication step. All other aspects are the same as in Example 1.

[0100] Comparative Example 2

[0101] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the hole injection layer does not include a P-type AlGaN / InN superlattice layer; correspondingly, the fabrication method also does not include the fabrication step of the P-type AlGaN / InN superlattice layer. All other aspects are the same as in Example 1.

[0102] Comparative Example 3

[0103] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the hole injection layer includes a Si3N4 layer, a P-type AlGaN layer, and a P-type InGaN layer sequentially stacked on the multiple quantum well layer, with the thickness of the P-type AlGaN layer being 25 nm; correspondingly, the fabrication method does not include the fabrication step of the first P-type AlInGaN layer. All other aspects are the same as in Example 1.

[0104] Comparative Example 4

[0105] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the hole injection layer includes a Si3N4 layer, an InN layer, and a P-type InGaN layer sequentially stacked on the multiple quantum well layer, with the InN layer having a thickness of 7.5 nm; correspondingly, the fabrication method does not include the fabrication step of the first P-type AlInGaN layer. All other aspects are the same as in Example 1.

[0106] Comparative Example 5

[0107] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the hole injection layer does not include a P-type InGaN layer; correspondingly, the fabrication method also does not include the fabrication step of the P-type InGaN layer. All other aspects are the same as in Example 1.

[0108] Performance testing:

[0109] The LED epitaxial wafers obtained in Examples 1 to 4 and Comparative Examples 1 to 5 were fabricated into 10mil×24mil chips and tested at 120mA / 60mA current. The luminous efficacy improvement rate of Examples 1 to 4 and Comparative Examples 2 to 5 compared with Comparative Example 1 was calculated, and the results are shown in Table 1.

[0110] Table 1. Photoelectric performance test results of LED epitaxial wafers

[0111]

[0112]

[0113] As can be seen from the table, the hole injection layer structure of the present invention can effectively improve the luminous efficiency of LEDs.

[0114] The above description represents the preferred embodiments of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention.

Claims

1. A light-emitting diode epitaxial wafer, characterized in that, The device includes a substrate and a buffer layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, a hole injection layer, an electron blocking layer, and a P-type GaN layer sequentially stacked on the substrate. The hole injection layer includes a Si3N4 layer, a P-type AlGaN / InN superlattice layer, and a P-type InGaN layer sequentially stacked on the multiple quantum well layer. The P-type AlGaN / InN superlattice layer includes periodically alternating layers of P-type AlGaN layers and InN layers. The growth period of the p-type AlGaN / InN superlattice layer is 1~20, the thickness of the p-type AlGaN layer is 1nm~50nm, the Al composition ratio is 0.01~0.5, and the Mg doping concentration is 1×10⁻⁶. 18 cm -3 ~1×10 20 cm -3 The thickness of the InN layer is 0.5nm to 5nm.

2. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The thickness of the Si3N4 layer is 1nm to 10nm.

3. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The thickness of the p-type InGaN layer is 5 nm to 100 nm, the In composition ratio is 0.01 to 0.3%, and the Mg doping concentration is 1 × 10⁻⁶. 19 cm -3 ~1×10 21 cm -3 .

4. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The electron blocking layer is an AlInGaN layer with a thickness of 10nm~40nm, an Al composition ratio of 0.01~0.1%, and an In composition ratio of 0.01~0.2%.

5. A method for preparing a light-emitting diode epitaxial wafer, used to prepare a light-emitting diode epitaxial wafer as described in any one of claims 1 to 4, characterized in that, Includes the following steps: A substrate is provided on which a buffer layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, a hole injection layer, an electron blocking layer, and a P-type GaN layer are sequentially grown. The hole injection layer comprises a Si3N4 layer, a P-type AlGaN / InN superlattice layer, and a P-type InGaN layer sequentially stacked on the multiple quantum well layer. The P-type AlGaN / InN superlattice layer comprises periodically alternating layers of P-type AlGaN and InN layers.

6. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 5, characterized in that, The growth temperature of the Si3N4 layer is 800℃~900℃, and the growth pressure is 50Torr~500Torr.

7. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 5, characterized in that, The growth temperature of the p-type AlGaN layer is 650℃~800℃, and the growth pressure is 50Torr~500Torr. The growth temperature of the InN layer is 650℃~800℃, and the growth pressure is 50Torr~500Torr.

8. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 5, characterized in that, The growth temperature of the P-type InGaN layer is 650℃~800℃, and the growth pressure is 50Torr~500Torr.

9. A light-emitting diode, characterized in that, The light-emitting diode includes a light-emitting diode epitaxial wafer as described in any one of claims 1 to 4.

Citation Information

Patent Citations

  • Light-emitting diode

    CN103137811A

  • Semiconductor light emitting device

    JP2004006468A