A hollow yolk structure cobalt-iron alloy / sulfide composite catalyst, and a preparation method and application thereof
By synthesizing a cobalt-iron alloy/sulfide composite catalyst with a hollow yolk structure, the problems of complex synthesis and high cost of cobalt-iron-based catalysts have been solved, enabling efficient applications in water electrolysis for oxygen evolution and zinc-air batteries, exhibiting excellent electrochemical performance and stability.
Patent Information
- Application Number
- CN202410068130.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-17
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-01-17
AI Technical Summary
Existing cobalt-iron-based catalysts are complex to synthesize, costly, have poor conductivity, few active sites, and low activity, making them difficult to effectively replace noble metal catalysts, especially in the oxygen evolution reaction of water electrolysis.
A hollow yolk-structured cobalt-iron alloy/sulfide composite catalyst was synthesized using a hydrothermal method and CVD chemical vapor deposition. The cobalt-iron alloy was encapsulated by sulfur molecules to form a core-shell structure, which increased the surface area and active sites, and improved conductivity and stability.
It significantly improves the catalyst's reactivity and selectivity, reduces the overpotential of the oxygen evolution reaction, increases the efficiency of oxygen evolution in water electrolysis, and exhibits high voltage, high power density, and long-term stability in zinc-air batteries.
Smart Images

Figure CN117954641B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the fields of materials science and electrocatalysis technology, specifically relating to a hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst, its preparation method, and its application, particularly in zinc-air batteries. Background Technology
[0002] The advantage of electrochemical water splitting is that it converts renewable energy into pure hydrogen and oxygen, achieving efficient energy conversion and diversified applications. However, compared to the hydrogen evolution reaction (HER), the oxygen evolution reaction (OER) is more difficult due to its slow reaction speed. Therefore, developing a highly efficient OER catalyst to accelerate the reaction rate and reduce the voltage required for the reaction is crucial. Currently, commonly used commercial catalysts such as IrO2 and RuO2 possess high catalytic activity, corrosion resistance, high stability, and cost-effectiveness, making them suitable for electrochemical water splitting and other electrochemical reactions. However, their high price, limited reserves, and unstable structure severely limit their development and large-scale application in the field of water electrolysis catalysts. Therefore, there is an urgent need to develop abundant, inexpensive, highly efficient, and highly stable water electrolysis catalysts.
[0003] Earth contains abundant transition metal elements such as Co, Fe, Ni, Cu, and Mn. These elements can form transition metal-based materials, such as metal oxides, metal sulfides, phosphides, and hydroxides. In recent years, in-depth research has been conducted on these materials, with the hope of using them to replace traditional noble metal-based catalysts and become highly efficient catalysts for the electrolysis of water for oxygen and hydrogen evolution.
[0004] Among them, compounds based on transition metals such as Co, Fe, and Ni have been widely studied as catalysts for the oxygen evolution reaction (OER) in alkaline electrolytes. However, the currently reported synthesis methods for cobalt-iron system materials have some limitations, such as complex processes, high costs, and high energy consumption. In addition, these materials have poor electrical conductivity, few active sites, and low activity, making them insufficient to compete with noble metal materials.
[0005] Therefore, researchers need to further improve synthesis methods, enhance the conductivity of transition metal-based materials, increase the number of active sites, and improve the activity of these active sites to make them more competitive catalysts. Research in this area is ongoing and is expected to yield breakthroughs, promoting the development of energy conversion and storage technologies.
[0006] For the reasons stated above, this application is hereby submitted. Summary of the Invention
[0007] In view of the above problems and defects, the objective of this invention is to provide a new solution, namely, a hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst, its preparation method, and its application. This catalyst forms a hollow yolk-structured catalyst by encapsulating the cobalt-iron alloy with sulfur molecules.
[0008] In other words, the hollow yolk structure of this invention can provide a larger surface area and more active sites, thereby enhancing the catalyst's reactivity and selectivity. By designing and preparing this catalyst, this invention can improve the conductivity, number of active sites, and activity of existing cobalt-iron-based catalysts, regulate pore size and pore structure to improve their catalytic performance in the oxygen evolution and hydrogen evolution reactions of water electrolysis, and improve their stability when applied to zinc-air batteries.
[0009] The research and application of the hollow yolk structure cobalt-iron alloy / sulfide composite catalyst of this invention is expected to provide an efficient and low-cost solution to replace traditional noble metal-based catalysts, and promote the development of electrochemistry and electrocatalysis.
[0010] In this invention, the inventors synthesized a hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst using a simple and energy-efficient hydrothermal method combined with CVD (chemical vapor deposition), resulting in a stable structure. Due to its hollow yolk structure, this structure provides a larger surface area and more active sites, thereby enhancing the catalyst's reactivity and selectivity. The presence of its cavity also effectively protects the catalyst's active sites from corrosion and damage by ambient gases such as oxygen and water vapor, thus enhancing its stability.
[0011] To achieve the first objective of this invention, the technical solution adopted by this invention is as follows:
[0012] A hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst, wherein the catalyst has a specific chemical composition of CoFe / Co-Fe-S, and the catalyst is a core-shell structured nanosphere, wherein the cobalt-iron alloy is the core and the cobalt-iron sulfide is the shell, forming a hollow yolk structure.
[0013] The second objective of this invention is to provide a method for preparing the hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst described above, the method specifically comprising the following steps:
[0014] (1) Mix divalent cobalt salt, divalent iron salt and surfactant according to the ratio, then add mixed solvent, and place the resulting mixture at 65-95℃ for constant temperature and stirring for 5-20 min; then add inorganic base to the reaction system, and continue to react at 65-95℃ with stirring for 20-60 min; then add hydrazine hydrate to the reaction system, and react at 65-95℃ with stirring for 1-4 h; after the reaction is completed, cool to room temperature, filter, wash and dry the resulting product to obtain cobalt-iron alloy precursor; wherein: the mixed solvent is composed of ethylene glycol and deionized water;
[0015] (2) According to the ratio, place the cobalt-iron alloy precursor and sulfur source described in step (1) into two crucibles at the downstream and upstream of the tube furnace, respectively; then heat the tube furnace to 300-900℃ at a rate of 5-10℃ / min and keep it at that temperature for 1-10 hours in an inert gas atmosphere, and then let it cool naturally to room temperature to obtain the hollow egg yolk structure cobalt-iron alloy / sulfide composite catalyst.
[0016] Furthermore, in the above technical solution, the divalent cobalt salt in step (1) can be any one or more of cobalt chloride, cobalt acetate, or cobalt nitrate.
[0017] Furthermore, in the above technical solution, the divalent iron salt in step (1) can be any one or more of ferrous oxide, ferrous nitrite, or ferrous sulfate.
[0018] Furthermore, in the above technical solution, the surfactant in step (1) is any one of polyvinylpyrrolidone, hexadecyltrimethylammonium bromide, and polyethoxyoctyl alcohol.
[0019] Furthermore, in the above technical solution, the total molar amount of the divalent cobalt salt and divalent iron salt in step (1) and the mass ratio of the surfactant are (1-10) mmol: (0.1-1) g.
[0020] Furthermore, in the above technical solution, the total molar amount of divalent cobalt salt and divalent iron salt in step (1) and the ratio of the amount of divalent cobalt salt to the mixed solvent are (1-10) mmol: (50-100) mL.
[0021] Furthermore, in the above technical solution, the molar ratio of the divalent cobalt salt and the divalent iron salt is 4:1.
[0022] Furthermore, in the above technical solution, the volume ratio of ethylene glycol to deionized water in step (1) is 4:1.
[0023] Furthermore, in the above technical solution, the total molar amount of the divalent cobalt salt and divalent iron salt in step (1) and the mass ratio of them to the inorganic base are (1-10) mmol: (3-10) g.
[0024] Furthermore, in the above technical solution, the inorganic base in step (1) is sodium hydroxide or potassium hydroxide.
[0025] Furthermore, in the above technical solution, the total molar amount of divalent cobalt salt and divalent iron salt in step (1) and the volume ratio of them to hydrazine hydrate are (1-10) mmol: (3-15) mL.
[0026] Furthermore, in the above technical solution, the sulfur source in step (2) is any one or more of sodium sulfide, hydrogen sulfide, sulfur powder, etc.
[0027] Furthermore, in the above technical solution, the mass ratio of the cobalt-iron alloy precursor to the sulfur source in step (2) is (1:5.25) to (1:12.25). That is, when the mass ratio of the precursor to the sulfur source is 1:5.25 to 1:12.25, cobalt-iron sulfides with different degrees of sulfidation can be prepared. For example, it can be 1:5.25, 1:7, 1:8.75, 1:10.5, 1:12.25, etc., but the performance is optimal when the mass ratio is 1:8.75.
[0028] Furthermore, in the above technical solution, the inert gas in step (2) is nitrogen or argon.
[0029] The third objective of this invention is to provide the application of the hollow yolk structure cobalt-iron alloy / sulfide composite catalyst described above in the catalytic electrolysis of water to produce oxygen.
[0030] A catalyst for catalytic electrolysis of water to produce oxygen, the catalyst comprising the hollow yolk structure cobalt-iron alloy / sulfide composite catalyst described above in this invention.
[0031] The fourth objective of this invention is to provide the application of the hollow yolk structure cobalt-iron alloy / sulfide composite catalyst described above in oxygen production in zinc-air batteries.
[0032] A catalyst for oxygen production in zinc-air batteries, the catalyst comprising the hollow yolk structure cobalt-iron alloy / sulfide composite catalyst described above in this invention.
[0033] The reaction mechanism of this invention and the roles of each raw material are as follows:
[0034] This invention uses divalent metal salts (including divalent cobalt and divalent iron salts) as the reaction metal source, employing low-valence metal salts to facilitate reduction to zero-valence metals; ethylene glycol is used in combination with an inorganic base to combine with metal ions to complete the nucleation process; a surfactant is used to adjust the size of the alloy nanospheres; hydrazine hydrate is used to ensure complete reduction of cobalt and ferrous ions to form the alloy. A sulfur source is used to form a stable hollow yolk structure.
[0035] The purpose of using a sulfur source to sulfide the cobalt-iron precursor in this invention is to obtain a catalyst with a cobalt-iron sulfide shell and a cobalt-iron core structure; and to regulate sulfur vacancies, which can improve the conductivity, reactivity and catalytic performance of the metal sulfide electrode, thereby improving electrochemical performance and catalytic activity.
[0036] The inert gas (including nitrogen or argon) used in this invention serves to expel and prevent oxygen from entering, thus preventing oxidation of the tubular heating element and the sample. These functions help protect the sample, improve the accuracy of experimental results, and optimize the reaction process and product quality.
[0037] This invention utilizes a hydrothermal synthesis of a cobalt-iron precursor, followed by sulfurization of the precursor with a sulfur source to create a hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst for oxygen evolution reaction (OER) in water electrolysis. This catalyst effectively and efficiently catalyzes the production of oxygen through water electrolysis and can be applied to zinc-air batteries. Compared to traditional cobalt-iron catalysts, the synthesized hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst offers advantages such as simple operation, low cost, high efficiency in catalytic OER, and structural stability. During catalyst synthesis, by encapsulating sulfides on the alloy to form a unique nanostructure, strong electron transport occurs between the sulfides and the cobalt-iron alloy, improving electron conductivity and the number of active sites, thereby significantly enhancing the electrocatalytic activity of the catalyst in the OER reaction. Furthermore, the hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst exhibits excellent performance in both liquid and solid zinc-air batteries, including high voltage, high power density, and long-term stability.
[0038] The catalyst prepared by this invention possesses high specific surface area, high electrical conductivity, and high catalytic activity, and can be used in the oxygen evolution reaction of water electrolysis. This invention also provides a method for preparing this catalyst, which includes the following steps:
[0039] (1) Cobalt-iron alloy precursors are synthesized by hydrothermal method using cobalt salts and iron salts as raw materials; (2) The cobalt-iron alloy precursors and sulfur source are subjected to sulfidation treatment in a nitrogen atmosphere to obtain a hollow cobalt-iron alloy / sulfide composite catalyst. The advantages of this invention are that, due to its hollow yolk structure, this structure can provide a larger surface area and active sites, thereby enhancing the reaction activity and selectivity of the catalyst. Due to the presence of its cavity, the active sites of the catalyst can be well protected and are not easily corroded and destroyed by environmental gases such as oxygen and water vapor, thereby enhancing its stability. The overpotential of the oxygen evolution reaction is reduced. The rapid charge transfer at the cavity structure layer of the catalyst of this invention can significantly improve the electrochemical kinetic process, thereby achieving efficient and stable water electrolysis and oxygen evolution. The catalyst synthesized by this invention has low energy consumption, simple process and low cost, which to a certain extent solves the problems of limited, high energy consumption, complex process and high cost of the synthesis method of cobalt-iron system materials. It can be applied to zinc-air batteries and exhibits excellent performance and stability, meeting the needs of long-term use of zinc-air batteries.
[0040] Compared with the prior art, the innovation and advantages of this invention are as follows:
[0041] (1) The experimental steps for preparing hollow egg yolk structure cobalt-iron alloy / sulfide composite catalyst of the present invention are simple, the reaction conditions are simple, the reaction time is short, the reaction temperature is low, and the energy consumption is low.
[0042] (2) In the cobalt-iron alloy / sulfide composite catalyst with a hollow yolk structure synthesized by hydrothermal method and sulfidation in this invention, the mass ratio of the precursor to the sulfur source is 1:5.25 to 1:12.25. When the mass ratio of the precursor to the sulfur source is 1:8.75, its oxygen evolution performance in water electrolysis is optimal, and it exhibits the best performance at 10 mA cm⁻¹. -2 The overpotential was only 263 mV, which is lower than the overpotentials of catalysts prepared under other mass ratios ((1:5.25); (1:7); (1:10.5); (1:12.25)) conditions: 291 mV, 275 mV, 289 mV and 334 mV.
[0043] (3) The hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst synthesized in this invention exhibits good stability at 10 mA cm⁻¹. -2 After prolonged electrolysis, the overpotential of the current density did not increase significantly: the overpotential decayed by only 13mV after 24 hours of electrolysis.
[0044] (4) The hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst synthesized in this invention, when used in zinc-air batteries, outperforms traditional commercial RuO2+Pt / C catalysts in charge-discharge performance tests, achieving a discharge power density of 127 mW / cm³. -2 Superior power density of 67 mW / cm³ compared to commercial RuO₂+Pt / C catalysts-2 .
[0045] (5) The hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst synthesized in this invention exhibits superior performance compared to traditional commercial RuO2+Pt / C catalysts in charge-discharge stability tests when used in zinc-air batteries. The charge-discharge current density is 50 mA cm⁻¹. -2 At that time, the charge-discharge cycle of the hollow yolk structure cobalt-iron alloy / sulfide composite catalyst reached 60 hours, which is better than the 46 hours of the commercial RuO2+Pt / C catalyst. Attached Figure Description
[0046] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0047] Figure 1 The XRD patterns of the catalysts synthesized from cobalt-iron alloy precursors and sulfur powder in different mass ratios in Examples 1-5 and Comparative Example 1 are shown.
[0048] Figure 2 Transmission electron microscope image of the hollow yolk structure catalyst prepared in Example 3 of this invention;
[0049] Figure 3 The catalysts synthesized under different raw material ratios in Examples 1-5, Comparative Examples 1 and 2 of this invention were tested at 5 mV / s. -1 Comparison of LSV curves obtained at different scan rates;
[0050] Figure 4 The graphs show the charge-discharge curves and power density test curves of the hollow yolk structure catalyst prepared in Example 3 in Application Example 1 of this invention during battery charge-discharge.
[0051] Figure 5 This is a stability curve of the hollow yolk structure catalyst prepared in Example 3 in Application Example 1 of the present invention during battery charge-discharge stability testing. Detailed Implementation
[0052] The present invention will be further described in detail below through implementation examples. These implementation examples are carried out based on the technology of the present invention. Detailed implementation methods and specific operating procedures are provided to illustrate the inventiveness of the present invention, but the scope of protection of the present invention is not limited to the following implementation examples.
[0053] This invention discloses a hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst and its preparation method, and applies this catalyst to the efficient oxygen evolution reaction (OER) of water electrolysis. First, a cobalt-iron alloy precursor is obtained using cobalt salt, ferrous salt, and hydrazine hydrate as metal sources and reducing agents. Then, the cobalt-iron alloy precursor and sulfur powder are subjected to sulfidation treatment in an inert gas atmosphere to obtain the hollow-structured cobalt-iron alloy / sulfide composite catalyst. This hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst not only has a simple and efficient synthesis method, but also exhibits high stability in electrocatalytic performance (overpotential decay of only 15 mV after 24 hours of electrolysis) and a low overpotential for the OER reaction (at 10 mA cm⁻¹). -2 With a current density of only 263mV, it can achieve efficient and stable oxygen evolution through water electrolysis.
[0054] The equipment and raw materials used in this invention are all commercially available or commonly used in the field. Unless otherwise specified, the methods in the following embodiments are conventional methods in the field.
[0055] Example 1
[0056] This embodiment presents a hollow yolk-structured cobalt-iron alloy / sulfide (CoFe / Co-Fe-S-1) composite catalyst, which is prepared by the following method, with the steps as follows:
[0057] (1) 1.8626 g (6.4 mmol) of cobalt nitrate hexahydrate, 0.4448 g (1.6 mmol) of ferrous sulfate heptahydrate, and 400 mg of polyvinylpyrrolidone (PVP) were placed in a three-necked flask. 80 mL of ethylene glycol and 20 mL of deionized water were added to the flask, and the flask was placed in an oil bath for heating. The oil bath temperature was kept constant at 85 °C with stirring. After stirring for 5 minutes, 6 g of sodium hydroxide was added. The temperature was kept constant at 85 °C for 20 minutes, and 8 mL of hydrazine hydrate (85 wt%, CAS No.: 10217-52-4) was slowly added dropwise using a pipette. Finally, the reaction was kept constant for 1 hour. After the reaction was completed, heating and stirring were stopped, and the product was cooled to room temperature and then filtered. The filtered product was first washed 2-3 times with distilled water, and then washed 2-3 times with anhydrous ethanol to obtain the cobalt-iron alloy precursor.
[0058] (2) Then, 100 mg of the cobalt-iron alloy precursor prepared in step (1) and 525 mg of sulfur powder were subjected to CVD chemical vapor deposition in a nitrogen atmosphere at 300 °C. The temperature was raised for 1 h at a rate of 5 °C / min, held for 1 h, and then allowed to cool naturally to room temperature to obtain a hollow cobalt-iron alloy / sulfide composite catalyst.
[0059] Example 2 CoFe / Co-Fe-S-2
[0060] This embodiment presents a hollow egg yolk structure catalyst with different degrees of sulfidation. The preparation method of the cobalt-iron based catalyst is the same as that in Example 1, except that the amount of sulfur powder in this embodiment is 700 mg, and the rest of the process is the same as that in Example 1.
[0061] Example 3 CoFe / Co-Fe-S-3
[0062] This embodiment presents a hollow egg yolk structure catalyst with different degrees of sulfidation. The preparation method of the cobalt-iron based catalyst is the same as that in Example 1, except that the amount of sulfur powder in this embodiment is 875 mg, and the rest of the process is the same as that in Example 1.
[0063] Example 4 CoFe / Co-Fe-S-4
[0064] This embodiment presents a hollow egg yolk structure catalyst with different degrees of sulfidation. The preparation method of the cobalt-iron based catalyst is the same as that in Example 1, except that the amount of sulfur powder in this embodiment is 1050 mg, and the rest of the process is the same as that in Example 1.
[0065] Example 5 CoFe / Co-Fe-S-5
[0066] This embodiment presents a hollow egg yolk structure catalyst with different degrees of sulfidation. The preparation method of the cobalt-iron based catalyst is the same as that in Example 1, except that the amount of sulfur powder in this embodiment is 1225 mg, and the rest of the process is the same as that in Example 1.
[0067] Comparative Example 1
[0068] This comparative example is a cobalt-iron alloy (Fe-Co) catalyst without sulfidation treatment. The preparation method of the cobalt-iron alloy catalyst is the same as that in Example 1, except that step (2) is not included in this comparative example.
[0069] Comparative Example 2
[0070] This comparative example provides a RuO2 catalyst.
[0071] Test Result Analysis:
[0072] Figure 1 The images show the XRD patterns of catalysts synthesized from cobalt-iron alloy precursors and sulfur powder in different mass ratios in Examples 1-5 and Comparative Example 1. Figure 1 It can be seen that without sulfidation, the product is only CoFe alloy. After sulfidation, FeS, CoS, and CoS2 peaks appeared, proving that sulfides were formed.
[0073] Figure 2The image shows a transmission electron microscope image of the catalyst synthesized from 100 mg of cobalt-iron alloy and 875 mg of sulfur powder in Example 3. The image clearly shows a hollow yolk bimetallic structure, proving the formation of the hollow yolk structure.
[0074] Application Examples
[0075] The catalysts synthesized in Examples 1-5 and Comparative Example 1 were used in the catalytic water electrolysis oxygen evolution reaction, and the specific application methods are as follows:
[0076] (1) Preparation of the catalytic electrode: First, 10 mg of catalyst powder, 980 μL of anhydrous ethanol, and 20 μL of 5% Nafion (perfluorosulfonic acid solution) reagent were mixed and sonicated for 1 h to form a uniform dispersion, which was then used to prepare the catalyst ink. Using a liquid gun, 50 μL of the catalyst dispersion was measured each time and evenly coated onto a 1 cm² area. 2 Each coating was applied to carbon paper and dried under an infrared lamp. After drying, the coating was repeated three times, consuming 200 μL of catalyst ink. The final working electrode was fabricated with a loading of 2 mg cm⁻¹. -2 1cm 2 Carbon paper.
[0077] (2) Construction of the electrochemical reaction system: In a three-electrode electrolytic cell, a carbon paper electrode loaded with the catalyst was used as the working electrode, a graphite rod as the auxiliary electrode (cathode), and an Ag / AgCl electrode as the reference electrode. 1 MkOH solution was used as the electrolyte. The various properties of the catalyst were measured. Specifically, the three-electrode system was connected to an electrochemical workstation. First, the catalyst was activated by cyclic voltammetry (CV) (potential window 1.0–1.7 V, vs. RHE) at a scan rate of 50 mV / s. -1 Until the CV curve reaches a stable state, the linear sweep voltammetry (LSV) method is used to scan at a rate of 5 mV / s within the same potential window. -1 LSV polarization curves of catalysts with different metal ratios were obtained through testing. The LSV curves of different samples were converted into Tafel curves to analyze their Tafel slopes and explore their underlying catalytic mechanisms. Finally, the sample with the best performance was subjected to stability testing (24 h) using the chronopotential (CP) method, with the current density set to a standard 10 mA / cm². -2 .
[0078] (3) The zinc-air battery was assembled using a specific mold, with 6M KOH and 0.2M C4H6O4·2H2O as the electrolyte, a zinc sheet as the negative electrode, and carbon paper as the positive electrode, with one side in contact with the electrolyte and the other side exposed to air. 25ml of electrolyte was added to construct the zinc-air battery. Its charge-discharge curve and open-circuit voltage stability were measured using an electrochemical workstation. Stability and charge-discharge specific capacity were tested using a blue electric channel.
[0079] Figure 3 The composite catalysts obtained by sulfiding 100 mg of cobalt-iron alloy precursor with 525 mg, 700 mg, 875 mg, 1050 mg, and 1225 mg of precursor in Examples 1-5, respectively, and the catalysts of Comparative Examples 1 and 2, during the electrolysis of water for oxygen evolution, showed a 5 mV / s ratio. -1 The LSV curve comparison chart was obtained at the scan rate, from Figure 3 The graph shows the relationship between current density and potential (relative to reversible hydrogen electrode vs. RHE) for different samples. Example 3 of this invention exhibits a smaller overpotential at the same current density, such as at 10 mA / cm². -2 At that time, the overpotential of the Co-Fe-S-3 hollow yolk structure catalyst was only 263 mV, significantly lower than the overpotentials of other samples (CoFe alloy, CoFe / Co-Fe-S-1, CoFe / Co-Fe-S-2, CoFe / Co-Fe-S-4, CoFe / Co-Fe-S-5, and the commercial OER catalyst RuO2) of 317 mV, 291 mV, 275 mV, 289 mV, 320 mV, and 335 mV, respectively, and superior to the commercial catalyst. CoFe / Co-Fe-S-1 and CoFe / Co-Fe-S-5, however, exhibited significant catalytic inertness, producing relatively low current densities. This indicates that the catalyst prepared in this invention at this ratio has better oxygen evolution performance in water electrolysis.
[0080] Figure 4 The application of the hollow cobalt-iron alloy / sulfide composite catalyst with a mass ratio of CoFe alloy to sulfur powder of 1:8.75 in zinc-air batteries was investigated. In the battery discharge power density test, the (CoFe / Co-Fe-S-3+RuO2) catalyst exhibited a higher power density than the (Pt / C+RuO2) catalyst, reaching 127 Mw / cm². -2 It is far greater than that of commercially available (Pt / C+RuO2) catalysts.
[0081] Figure 5 To investigate the application of the hollow cobalt-iron alloy / sulfide composite catalyst synthesized at a CoFe alloy to sulfur powder mass ratio of 1:8.75 in zinc-air batteries, the battery's cycle stability was tested at a constant 50 mA / cm². -2At the specified current, the (CoFe / Co-Fe-S-3+RuO2) catalyst exhibits longer stability than the (Pt / C+RuO2) catalyst, up to 60 h, which is greater than the 45 h stability of the commercial (Pt / C+RuO2) catalyst.
Claims
1. A hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst, characterized in that: The catalyst has a specific chemical composition of CoFe / Co-Fe-S. The catalyst is a core-shell structured nanosphere, wherein the cobalt-iron alloy is the core and the cobalt-iron sulfide is the shell, forming a hollow yolk structure.
2. The preparation method of the hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst according to claim 1, characterized in that: The method specifically includes the following steps: (1) Mix divalent cobalt salt, divalent iron salt and surfactant according to the ratio, then add mixed solvent, and place the resulting mixture at 65-95 ℃ for constant temperature stirring for 5-20 min; then add inorganic base to the reaction system, and continue to react at 65-95 ℃ with constant temperature stirring for 20-60 min; then add hydrazine hydrate to the reaction system, and react at 65-95 ℃ with constant temperature stirring for 1-4 h; after the reaction is completed, cool to room temperature, filter, wash and dry the obtained product to obtain cobalt-iron alloy precursor; wherein: the mixed solvent is composed of ethylene glycol and deionized water; (2) According to the ratio, place the cobalt-iron alloy precursor and sulfur source described in step (1) into two crucibles at the downstream and upstream of the tube furnace respectively; then heat the tube furnace to 300-900 °C at a rate of 5-10 °C / min and keep it at the temperature for 1-10 hours in an inert gas atmosphere, and then let it cool naturally to room temperature to obtain the hollow egg yolk structure cobalt-iron alloy / sulfide composite catalyst.
3. The method according to claim 2, characterized in that: The total molar amount of the divalent cobalt salt and divalent iron salt in step (1) and the mass ratio of the surfactant are (1~10) mmol: (0.1~1) g.
4. The method according to claim 2, characterized in that: The molar ratio of the divalent cobalt salt and the divalent iron salt is 4:
1.
5. The method according to claim 2, characterized in that: The total molar amount of the divalent cobalt salt and divalent iron salt in step (1), and the volume ratio of them to hydrazine hydrate, is (1~10) mmol: (3~15) mL.
6. The method according to claim 2, characterized in that: The mass ratio of the cobalt-iron alloy precursor to the sulfur source in step (2) is (1:5.25) to (1:12.25).
7. The application of the hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst according to claim 1 or the hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst prepared by the method according to any one of claims 2-6 in the catalytic electrolysis of water to produce oxygen.
8. The application of the hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst according to claim 1 or the hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst prepared by the method according to any one of claims 2-6 in oxygen production in zinc-air batteries.
9. A catalyst, characterized in that: The catalyst comprises a hollow yolk-structured cobalt-iron alloy / sulfide composite catalyst prepared by the method of any one of claims 2-6.