A separator, a method of manufacturing the same, an electrode assembly, and a secondary battery
By setting coatings with different particle sizes in different areas of the lithium-ion battery separator, the problem of adhesion difference between the electrode thinning area and the separator is solved, and the adhesion strength between the separator and the electrode is consistent, avoiding edge lithium plating and electrode wrinkling, and improving battery performance and production stability.
Patent Information
- Application Number
- CN202410083783.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-19
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-01-19
AI Technical Summary
Differences in adhesion between the thinned area of the lithium-ion battery electrode and the separator lead to problems such as edge lithium plating and electrode wrinkling, which affect the industrialization of lithium batteries.
Flat area coating and thinned area coating are set in different areas of the base membrane. Adhesives with different particle sizes are used to match the flat area and thinned area of the electrode respectively. By adjusting the adhesive particle size and coating thickness, the bonding strength between the separator and the electrode is ensured to be consistent.
It eliminates the adhesion difference between the electrode thinning area and the separator, avoids lithium deposition and wrinkling at the electrode edges, and improves the electrical performance and production stability of lithium batteries.
Smart Images

Figure CN117954776B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery technology, and more specifically, to a separator and its preparation method, an electrode assembly, and a secondary battery. Background Technology
[0002] With the rapid development of the new energy vehicle industry, lithium-ion batteries, as one of the main power sources, have a huge market prospect, but this also places higher demands on their manufacturing. In the lithium battery coating process, to avoid the "thick edge" phenomenon caused by the fluid characteristics of the slurry, the thickness of the auxiliary material layer in the electrode edge area is usually thinned, creating a thinned electrode zone. However, due to the difference in adhesion between the thinned electrode zone and the normal area and the separator, problems such as edge lithium plating and electrode wrinkling can occur, thus hindering the industrialization of the new energy industry. Summary of the Invention
[0003] The problem this invention aims to solve is how to address the issues of lithium deposition and interface wrinkling in battery electrode thinning areas.
[0004] To solve at least one of the above problems, the present invention provides a method for preparing a diaphragm, comprising:
[0005] Prepare the first slurry and the second slurry respectively;
[0006] The first slurry and the second slurry are respectively coated on different areas of the base film to form a flat area coating and a thinned area coating;
[0007] A diaphragm is obtained based on the base film, the flat area coating, and the thinned area coating.
[0008] Optionally, the flat zone coating is made of a flat zone adhesive, and the thinned zone coating is made of a thinned zone adhesive, wherein the average particle size of the flat zone adhesive is smaller than the average particle size of the thinned zone adhesive.
[0009] Optionally, the flat area adhesive includes a first adhesive and a third adhesive, and the thinned area adhesive includes a second adhesive and a fourth adhesive. The first adhesive and the second adhesive are disposed on the front side of the base film, and the average particle size of the first adhesive is smaller than the average particle size of the second adhesive. The third adhesive and the fourth adhesive are disposed on the back side of the base film, and the average particle size of the third adhesive is smaller than the average particle size of the fourth adhesive.
[0010] Optionally, the ratio of the average particle size of the second adhesive to the average particle size of the first adhesive is 2-4, and / or the ratio of the average particle size of the fourth adhesive to the average particle size of the third adhesive is 2-6.
[0011] Optionally, the average particle size of the first adhesive is 0.1-0.5 μm, the average particle size of the second adhesive is 1.0-2.0 μm; and / or, the average particle size of the third adhesive is 0.5-3.5 μm, and the average particle size of the fourth adhesive is 4.0-8.0 μm.
[0012] Optionally, the first adhesive comprises one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polytetrafluoroethylene, copolymer derivatives of polyvinylidene fluoride, and copolymer derivatives of tetrafluoroethylene; and the second adhesive comprises one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polytetrafluoroethylene, copolymer derivatives of polyvinylidene fluoride, and copolymer derivatives of tetrafluoroethylene; and / or,
[0013] The third adhesive includes one or more of polyethylene glycol, polymethyl acrylate, polymethyl methacrylate, polyethyl methacrylate, polybutyl methacrylate, polyacrylic acid, polyvinyl acetate, acrylate copolymers, styrene-butadiene latex, styrene-acrylic latex, polyvinyl alcohol, and sodium carboxymethyl cellulose. The fourth adhesive includes one or more of polyethylene glycol, polymethyl acrylate, polymethyl methacrylate, polyethyl methacrylate, polybutyl methacrylate, polyacrylic acid, polyvinyl acetate, acrylate copolymers, styrene-butadiene latex, styrene-acrylic latex, polyvinyl alcohol, and sodium carboxymethyl cellulose.
[0014] Optionally, before coating the first slurry and the second slurry onto different areas of the base film, the method further includes coating the surface of the base film with a ceramic slurry to obtain a ceramic coating.
[0015] The present invention also provides a diaphragm, which is prepared by the diaphragm preparation method described above.
[0016] The present invention also provides an electrode assembly, including a positive electrode, a negative electrode and a diaphragm as described above, wherein the diaphragm is disposed between the positive electrode and the negative electrode.
[0017] The present invention also provides a secondary battery, including the electrode assembly described above.
[0018] This invention provides a separator with different coatings in different regions of the base film, specifically a flat region coating and a thinned region coating. This results in a separator with different coatings for different regions. When applied to a secondary battery, the different coatings on the separator can be matched to different regions of the electrode. For example, for an electrode with flat and thinned regions, the flat region coating of the separator can be connected to the flat region of the electrode, and the thinned region coating of the separator can be connected to the thinned region of the electrode. This matching between the separator and different regions of the electrode eliminates the difference in adhesion between the flat and thinned regions of the electrode and the separator, resulting in better adhesion between the thinned region of the electrode and the separator. This shortens the transport path of lithium ions in the electrode sheet, thereby slowing down lithium deposition at the electrode edge. Simultaneously, it improves the consistency of the adhesion strength between the separator and the flat region of the electrode and the adhesion strength between the thinned region of the electrode, preventing electrode wrinkling during lithium battery production. Attached Figure Description
[0019] Figure 1 This is a schematic diagram of the diaphragm structure in an embodiment of the present invention. Figure 1 ;
[0020] Figure 2 This is a schematic diagram of the diaphragm structure in an embodiment of the present invention. Figure 2 ;
[0021] Figure 3 This is a schematic diagram of the negative electrode structure in an embodiment of the present invention;
[0022] Figure 4 This is a schematic diagram of the diaphragm structure in an embodiment of the present invention. Figure 3 ;
[0023] Figure 5 This is a schematic diagram of the electrode assembly in an embodiment of the present invention;
[0024] Figure 6 This is a schematic diagram illustrating the matching of the diaphragm and the positive and negative electrode regions in an embodiment of the present invention.
[0025] Explanation of reference numerals in the attached figures:
[0026] 1. Diaphragm; 11. Base film; 12. Flat area coating; 13. Thinned area coating; 14. Ceramic coating;
[0027] 2. Negative electrode; 21. Negative electrode current collector; 22. Negative electrode active material layer; 23. Negative electrode flat region; 24. Negative electrode thinning region;
[0028] 3. Positive electrode; 31. Positive electrode current collector; 32. Positive electrode active material layer; 33. Positive electrode flat region; 34. Positive electrode thinning region;
[0029] 101. First adhesive coating; 102. Second adhesive coating. Detailed Implementation
[0030] During the coating process of positive and negative electrodes in lithium-ion batteries, a sudden increase in thickness at the edges of the coated electrodes due to the fluid characteristics of the slurry is known as the "thick edge" phenomenon. For example, uneven slurry flow, unstable coating equipment, excessively fast or slow coating speed, or uneven coating pressure can generate surface tension, leading to excessive slurry accumulation at the electrode edges during coating, thus forming the thick edge phenomenon. The formation of thick edges is detrimental to improving the stability of the battery manufacturing process and the consistency of battery performance.
[0031] In related technologies, shims are typically used to address the issue of thick edges. Specifically, during the coating process, shims help adjust the working state of the coating equipment, ensuring more uniform flow of the slurry and thus reducing the occurrence of thick edges. For example, shims are added to parts of the coating equipment such as rollers or scrapers to adjust their position and gap, ensuring that the thickness of the auxiliary material layer in the edge area of the coated electrode is thinner than that in the normal area, thereby alleviating or eliminating the phenomenon of sudden thickness increases at the edges.
[0032] However, thinning the electrode sheet introduces new problems. For example, during the hot-pressing process of electrode assembly, the thinned area often doesn't press sufficiently, resulting in poorer adhesion of the diaphragm compared to the normal area. This leads to a difference in peel force between the thinned and normal areas. Here, the normal area of the electrode sheet is a flat area where the thickness of the electrode active material layer remains within a preset range. In other words, it can be considered essentially constant, or fluctuates only within a small range, while remaining largely unchanged overall. The thinned area of the electrode sheet is the region where the electrode edge is thinned to avoid thick edges. In this area, the thickness of the electrode active material layer gradually decreases from the flat area away from it. Figure 3 Taking the negative electrode 2 as an example, the cross-section of the flat negative electrode region 23 on the left can be regarded as a rectangle, while the negative electrode thinning region 24 on its right shows a thinning trend from left to right, and the whole can be trapezoidal or triangular. Correspondingly, the area between the negative electrode thinning region 24 and the base film 11 is larger.
[0033] This invention provides a separator and its preparation method, an electrode assembly, and a secondary battery, aiming to mitigate the problem of lithium deposition in the thinned area of the electrode during battery cell cycling. At the same time, by improving the more uniform adhesion between the separator and the electrode, it avoids the interface wrinkling phenomenon in the manufacturing process of lithium-ion batteries.
[0034] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0035] A method for preparing a diaphragm according to an embodiment of the present invention includes:
[0036] Prepare the first slurry and the second slurry respectively;
[0037] The first slurry and the second slurry are respectively coated on different areas of the base film 11 to form a flat area coating 12 and a thinned area coating 13;
[0038] A diaphragm is obtained based on the base film 11, the flat area coating 12, and the thinned area coating 13.
[0039] In this embodiment, different coatings are applied to different regions of the base film 11, specifically a flat region coating 12 and a thinned region coating 13, thereby obtaining a diaphragm with different coatings corresponding to different regions. Figure 1 , Figure 2 Here, the differences in coatings can be reflected in variations in parameters such as coating material, thickness, and roughness, as well as differences in the adhesives used, including the type and particle size of the adhesive. It should be understood that when a separator is used in a secondary battery, it is assembled together with the positive and negative electrode plates. Figure 5 The coating on the base film is mainly used to bond the electrode sheets; therefore, the main component of the coating is the adhesive. Differences in coating materials primarily refer to differences in the type and particle size of the adhesive used. In this embodiment, the main difference lies in the particle size of the adhesive used in the coating, resulting in a flat zone coating and a thinned zone coating on the base film surface. It should also be noted that the term "thinned zone coating" does not refer to a thinner coating thickness in that area, but rather is a name used to correspond to the electrode thinning zone; that is, the coating corresponding to the electrode thinning zone is called the thinned zone coating, and the coating corresponding to the electrode flat zone is called the flat zone coating.
[0040] Therefore, when applying separators to applications such as secondary batteries, different coatings on the separator can be matched to different regions of the electrode. For example, for electrodes with flat and thinned regions, the coating for the flat region of the separator can be connected to the flat region of the electrode, and the coating for the thinned region of the separator can be connected to the thinned region of the electrode. This matching between the separator and different regions of the electrode eliminates the difference in adhesion between the flat and thinned regions of the electrode and the separator, while also ensuring better consistency in the adhesion strength between the separator and the flat and thinned regions of the electrode, thus preventing electrode wrinkling during lithium battery production.
[0041] In some embodiments, the flat area coating 12 is made of a flat area adhesive, the thinned area coating 13 is made of a thinned area adhesive, and the average particle size of the flat area adhesive is smaller than the average particle size of the thinned area adhesive.
[0042] In this embodiment, the flat area coating 12 is made of a flat area adhesive with a small particle size, and the thinned area coating 13 is made of a thinned area adhesive with a larger particle size. When the separator is applied to a secondary battery, the flat area coating 12 on the separator is used to match the flat area of the electrode, and the thinned area coating 13 is used to match the thinned area of the electrode. Thus, by adjusting the particle size of the adhesive that contacts different areas (flat area and thinned area) of the separator and the electrode, better consistency in the bonding strength between the separator and the flat area of the electrode and the bonding strength between the thinned area of the electrode can be ensured, thereby avoiding the phenomenon of electrode wrinkling during the lithium battery production process (formation, capacity testing, etc.). At the same time, by matching a coating layer with a larger particle size to the separator area corresponding to the thinned area of the electrode and a coating layer with a smaller particle size to the separator area corresponding to the flat area of the electrode, the difference in adhesion between the flat area and the thinned area of the electrode and the separator can be eliminated, resulting in a better adhesion effect between the thinned area of the electrode and the separator, shortening the transport path of lithium ions in the electrode electrode, thereby slowing down lithium deposition at the electrode edge. In addition, by adjusting the particle size, compared with adjusting the coating thickness, the air permeability of the coating can be guaranteed, and the poor air permeability of the coating can prevent the membrane from closing pores during the cycle, which would increase the transmission impedance of lithium ions between the membrane and the electrode and thus lead to lithium deposition at the cell interface.
[0043] Therefore, this embodiment, by using adhesives with different particle sizes in different areas of the separator coating, can reduce the difference in adhesion between different areas of the electrode and the separator, and ensure good air permeability of the separator, thereby avoiding edge lithium plating and electrode wrinkling, resulting in better battery electrical performance. Furthermore, it can avoid the problem of the electrode core being too soft after hot pressing, ensuring consistent cell hardness and facilitating electrode core assembly.
[0044] In some embodiments, the flat area adhesive includes a first adhesive and a third adhesive, and the thinned area adhesive includes a second adhesive and a fourth adhesive. The first and second adhesives are disposed on the front side of the base film 11, and the average particle size of the first adhesive is smaller than the average particle size of the second adhesive. The third and fourth adhesives are disposed on the back side of the base film 11, and the average particle size of the third adhesive is smaller than the average particle size of the fourth adhesive.
[0045] In this embodiment, to solve the problem of wrinkling of the negative electrode sheet, a coating is provided on both the front and back sides of the base film 11. Figure 2Each coating includes a flat area coating and a thinned area coating. To distinguish them, the flat area coating on the front side of the base membrane 11 is made of a first adhesive, the thinned area coating on the front side of the base membrane 11 is made of a second adhesive, the flat area coating on the back side of the base membrane 11 is made of a third adhesive, and the thinned area coating on the back side of the base membrane 11 is made of a fourth adhesive. Thus, for the connection between the separator 1 and the positive electrode 3, a first adhesive with a smaller particle size is coated on the base membrane 11 corresponding to the flat area 33 of the positive electrode to form a flat area coating 12, and a second adhesive with a larger particle size is coated on the base membrane 11 corresponding to the thinned area 34 of the positive electrode to form a thinned area coating 13. By increasing the particle size, the thinning thickness of the thinned area 34 of the positive electrode is compensated, so that the adhesion between the positive electrode 3 and the separator 1 maintains a high degree of consistency. Similarly, for the connection between the separator 1 and the negative electrode 2, a third adhesive with a smaller particle size is coated on the base film 11 corresponding to the flat region 23 of the negative electrode to form a flat region coating 12, and a fourth adhesive with a larger particle size is coated on the base film 11 corresponding to the thinned region 24 of the negative electrode to form a thinned region coating 13. By increasing the particle size, the thinning thickness of the thinned region 24 of the negative electrode is compensated, so that the adhesion between the negative electrode 2 and the separator 1 maintains a high degree of consistency.
[0046] Understandable, such as Figure 3 As shown, the positive electrode 3 includes a positive current collector 31 and a positive active material layer 32 disposed on the surface of the positive current collector 31, and the negative electrode 2 includes a negative current collector 21 and a negative active material layer 22 disposed on the surface of the negative current collector 21. Due to the thickness variation of the positive active material layer 32, the positive electrode 3 includes a positive flat region 33 and a positive thinning region 34. Figure 6 The thickness of the positive electrode active material layer 32 within the positive electrode flat region 33 is constant, while the thickness of the positive electrode active material layer 32 within the positive electrode thinning region 34 decreases from the positive electrode flat region 33 away from it. Due to the change in the thickness of the negative electrode active material layer 22, the negative electrode 2 includes a negative electrode flat region 23 and a negative electrode thinning region 24. Figure 6 The thickness of the negative electrode active material layer 22 is constant within the negative electrode flat region 23, while the thickness of the negative electrode active material layer 22 decreases from the negative electrode flat region 23 away from it. For ease of description, the coating on the base film 11 that is connected to the positive electrode 3 is referred to as the first adhesive coating 101. Figure 6 The coating on the base film 11 that is connected to the negative electrode 2 is called the second adhesive coating 102. Figure 6 The first adhesive coating 101 and the second adhesive coating 102 are referred to as adhesive coatings. The first adhesive coating 101 includes a first adhesive and a second adhesive, and the second adhesive coating 102 includes a third adhesive and a fourth adhesive.
[0047] In this embodiment, a first adhesive coating 101 and a second adhesive coating 102 connected to the positive and negative electrodes are respectively provided on both sides of the diaphragm. A coating layer with larger particles is coated on the diaphragm corresponding to the thinned area of the positive and negative electrode sheets to increase the thickness of the diaphragm adhesive layer, thereby compensating for the thickness of the thinned area of the electrode sheets and ensuring that the thinned area of the positive and negative electrode sheets has the same peel force level as the normal flat area.
[0048] In some embodiments, to better match the thickness compensation of the thinned zone, this embodiment also studies the particle size ratio. Specifically, the ratio of the average particle size of the second adhesive to the average particle size of the first adhesive is set to 2-4, and / or the ratio of the average particle size of the fourth adhesive to the average particle size of the third adhesive is set to 2-6. By designing the particle size ratio of the adhesive within the above range, the consistency of the bonding effect can be better guaranteed, which is more conducive to improving the performance of the battery cell.
[0049] In some embodiments, the inventors, through extensive experimental research, discovered that screening the particle size of the adhesive can further ensure the battery cell has good electrical performance. Specifically, the average particle size of the first adhesive is 0.1-0.5 μm, the average particle size of the second adhesive is 1.0-2.0 μm, the average particle size of the third adhesive is 0.5-3.5 μm, and the average particle size of the fourth adhesive is 4.0-8.0 μm.
[0050] In some embodiments, the first adhesive includes one or more of polyvinylidene fluoride (PVDF), PVDF-hexafluoropropylene copolymer, polytetrafluoroethylene (PTFE), copolymer derivatives of PVDF, and copolymer derivatives of tetrafluoroethylene, and the second adhesive includes one or more of PVDF, PVDF-hexafluoropropylene copolymer, PTFE, copolymer derivatives of PVDF, and copolymer derivatives of tetrafluoroethylene. Here, the first adhesive and the second adhesive may be the same or different.
[0051] The third adhesive includes one or more of polyethylene glycol, polymethyl acrylate, polymethyl methacrylate, polyethyl methacrylate, polybutyl methacrylate, polyacrylic acid, polyvinyl acetate, acrylate copolymers, styrene-butadiene latex, styrene-acrylic latex, polyvinyl alcohol, and sodium carboxymethyl cellulose. The fourth adhesive includes one or more of polyethylene glycol, polymethyl acrylate, polymethyl methacrylate, polyethyl methacrylate, polybutyl methacrylate, polyacrylic acid, polyvinyl acetate, acrylate copolymers, styrene-butadiene latex, styrene-acrylic latex, polyvinyl alcohol, and sodium carboxymethyl cellulose. Here, the third and fourth adhesives can be the same or different.
[0052] In some embodiments, before coating the first slurry and the second slurry onto different regions of the base film 11, the method further includes: coating the surface of the base film 11 with a ceramic slurry to obtain a ceramic coating 14. Figure 4 That is, the prepared diaphragm also includes a ceramic coating 14, which is disposed between the base membrane 11 and the adhesive coating.
[0053] At high temperatures, thermal runaway may occur inside lithium batteries, causing the battery temperature to rise too quickly. The presence of the ceramic coating 14 provides additional thermal stability, suppressing the occurrence of thermal runaway. Furthermore, in the event of thermal runaway, the ceramic coating 14 can act as a heat insulation layer, slowing down the rate of heat dissipation. Therefore, the presence of the ceramic coating 14 can improve the thermal stability of the separator.
[0054] In some embodiments, the ceramic coating 14 contains inorganic materials, including one or more of alumina, boehmite, silicon dioxide, calcium sulfate, magnesium sulfate, and magnesium hydroxide.
[0055] These inorganic materials typically have high thermal stability, enabling them to maintain structural stability at high temperatures, which in turn helps improve the thermal stability of the diaphragm.
[0056] Another embodiment of the present invention provides a diaphragm prepared by the diaphragm preparation method described above. The diaphragm includes a base film 11 and an adhesive coating disposed on the surface of the base film 11. The adhesive coating includes a flat area coating 12 and a thinned area coating 13.
[0057] In some embodiments, the adhesive coating has a coverage of 5%-80% on the surface of the base film 1.
[0058] It should be understood that when applying the adhesive coating to the surface of the base film 11, it is possible to apply the coating only to the front side of the base film 11. Figure 1 Alternatively, it can be coated on both the front and back sides of the base film 11. Figure 2As mentioned above, to avoid wrinkling of the negative electrode sheet, this embodiment preferably coats both the front and back sides of the base film 11 with an adhesive coating. However, when coating an adhesive coating on a surface, it is generally not fully covered, as full coverage is not conducive to electrolyte wetting. Therefore, the adhesive coating on the surface of the base film is usually distributed in an island-like pattern, or a dotted or discontinuous distribution. It can be understood that the greater the density of the island distribution of the adhesive coating on the same surface, the greater the coverage of the adhesive coating on that surface, and vice versa. A lower coverage rate may reduce the bonding strength and stability of the separator, leading to problems such as delamination, breakage, or electrolyte penetration during use, thereby affecting the safety performance of the battery. A higher coverage rate will also increase the thickness and weight of the separator, thereby affecting the energy density and cost of the battery. Furthermore, an excessively high coverage rate may also affect the gas permeability and ion transport performance of the separator, thereby affecting the charge and discharge performance of the battery. Taking all factors into consideration, the coverage rate of the adhesive coating on the surface of the base film 11 is designed within the above-mentioned range to ensure that the overall performance of the battery can be effectively improved.
[0059] In at least one preferred embodiment, the adhesive coating has a coverage of 30%-60% on the surface of the base film 11.
[0060] In some embodiments, the thickness of the adhesive coating is 0.5-10 μm.
[0061] Thin adhesive coatings (below 0.5 μm) may result in insufficient adhesive strength, affecting the bonding performance between the base membrane 11 and the adhesive coating. Thicker adhesive coatings (above 10 μm) may affect the thickness and permeability of the diaphragm, thus requiring the design of an appropriate thickness to balance the bonding strength and permeability of the diaphragm. It should be noted that since the adhesive coating includes a flattened area coating 12 and a thinned area coating 13, the thickness limitation here only characterizes the adhesive coating as a whole. It can be understood that the thickness of the thinned area coating 13 generally needs to match the thickness of the electrode thinning area; that is, if the electrode thinning area is thin, the thickness of the thinned area coating will correspondingly increase to ensure that the thinned area coating 13 can fill the gap between the electrode thinning area and the diaphragm, guaranteeing the bonding consistency between the diaphragm and the electrode thinning area and the flattened area. Therefore, the overall thickness of the thinned area coating 13 is greater than the thickness of the flattened area coating 12.
[0062] Furthermore, it should be noted that since the flat area coating 12 corresponds to the flat area of the electrode and the thinning area coating 13 corresponds to the thinning area of the electrode, the lengths of the flat area coating 12 and the thinning area coating 13 can be determined according to the actual situation of the electrode. However, it is necessary to ensure that the length of the thinning area coating 13 is within a reasonable range. It should not be too large or too small. If it is too large, it will reduce the cell capacity. If it is too small, it will cause insufficient adhesion to the electrode. Here, in this embodiment, the length of the thinning area coating 13 is set to 5-15mm to meet the above requirements.
[0063] In some embodiments, the areal density of the adhesive coating is 0.2-2.0 g / m³. 2 .
[0064] By selecting an appropriate areal density, this embodiment can provide good bonding strength and ensure a firm connection between the base film 1 and the adhesive coating 2.
[0065] In some embodiments, the thickness of the base film 11 is 5-9 μm.
[0066] A thinner base film 11 can improve the permeability of lithium ions, which is beneficial to the charge and discharge performance of the battery. However, an excessively thin base film 11 may pose a risk of puncture or tearing. By setting the thickness of the base film 11 to 5-9 μm, it is possible to ensure that the base film 11 is not punctured while providing sufficient mechanical strength to ensure that the separator is not easily broken or deformed during battery assembly and use.
[0067] In some embodiments, the base membrane 11 includes one or more of polyethylene, polypropylene, PET nonwoven fabric, PVDF, and polyimide porous membrane.
[0068] In some embodiments, the porosity of the diaphragm is 40%-60%.
[0069] The aforementioned range of membrane porosity can promote lithium-ion transport within the membrane, improve the wettability of the electrolyte within the membrane, and ensure the mechanical strength of the membrane. In specific implementation, the porosity can be adjusted by selecting the base film 11 material or controlling parameters such as the thickness and composition of the adhesive coating to meet the needs of different lithium battery applications.
[0070] Another embodiment of the present invention provides an electrode assembly including a positive electrode 3, a negative electrode 2, and a separator 1 disposed between the positive electrode 3 and the negative electrode 2. The positive electrode 3 and the negative electrode 2 each include a flat region and a thinned region connected to each other. The separator 1 includes a base film 11 and an adhesive coating disposed on the surface of the base film 11. The adhesive coating includes a flat region coating 12 connected to the flat region and a thinned region coating 13 connected to the thinned region.
[0071] The method for preparing the electrode assembly includes:
[0072] A slurry of positive electrode active material is applied to positive electrode current collector 31 to prepare positive electrode 3; a slurry of negative electrode active material is applied to negative electrode current collector 21 to prepare negative electrode 2.
[0073] A first slurry and a second slurry are prepared respectively, and the first slurry and the second slurry are coated on different areas of the base film 11 to form a flat area coating 12 and a thinned area coating 13, thereby obtaining a diaphragm 1;
[0074] The positive electrode 3, the separator 1, and the negative electrode 2 are assembled together to obtain an electrode assembly.
[0075] In at least one embodiment, in the step of preparing the separator, a first adhesive slurry, a second adhesive slurry, a third adhesive slurry, and a fourth adhesive slurry are prepared respectively, and the first adhesive slurry, the second adhesive slurry, the third adhesive slurry, and the fourth adhesive slurry are coated on the first region, the second region, the third region, and the fourth region of the base film 11 respectively to obtain the separator; wherein, the first region corresponds to the positive electrode flat region 33, the second region corresponds to the positive electrode thinning region 34, the third region corresponds to the negative electrode flat region 23, and the fourth region corresponds to the negative electrode thinning region 24.
[0076] In at least one embodiment, the coating slurry is applied to the corresponding area of the base film 11 using a micro-grooving roller coating method.
[0077] This invention also provides a secondary battery, including the electrode assembly as described above, as well as an electrolyte and a battery casing. During battery assembly, the electrolyte and electrode assembly are placed into the battery casing, and the battery is sealed by processes such as sealing and welding to ensure that the electrolyte does not leak.
[0078] The present invention will now be described in detail through specific embodiments.
[0079] Example 1
[0080] This embodiment provides a secondary battery, the preparation method of which includes the following steps:
[0081] 1.1 Preparation of the positive electrode: The positive electrode selected in this embodiment is lithium iron phosphate, with the mass ratios of lithium iron phosphate, binder, and conductive carbon black being 94.5%, 3.0%, and 2.5%, respectively, and the areal density on one side being 164 g / m². 2 The designed compaction density is 2.5 g / cm³. 3 The positive electrode sheet is prepared by sequentially stirring, coating, and rolling.
[0082] 1.2 Preparation of the negative electrode: The selected negative electrode is artificial graphite. The mass ratios of artificial graphite, binder, dispersant, and conductive carbon black are 94.0%, 2.5%, 2.0%, and 1.5%, respectively, with a single-sided areal density of 76 g / m². 2 The designed compaction density is 1.5 g / cm³. 3 The negative electrode sheet is prepared by sequentially stirring, coating, and rolling.
[0083] 1.3 Preparation of the diaphragm: A coating slurry was prepared, comprising a first adhesive slurry, a second adhesive slurry, a third adhesive slurry, and a fourth adhesive slurry. The coating slurry was then applied to both sides of a PE substrate containing an inorganic material layer, with a thickness of 13 μm, using a micro-gravure roller coating method. The coating density was 1.0 g / m². 2 The thickness of the PE substrate is 9μm, and each side of the substrate is coated with 2μm of aluminum oxide. Therefore, the thickness of the PE substrate containing the inorganic material layer is 13μm.
[0084] 1.4 Cell Assembly: The prepared positive and negative electrode sheets and separators are cut and stacked, hot-pressed electrode tabs are welded, inserted into a square aluminum shell, baked, injected with electrolyte, packaged, left to stand, formed, aged at high temperature, capacity tested, and coated to obtain a secondary battery.
[0085] Examples 2-9
[0086] The differences between Examples 2-9 and Example 1 are shown in Table 1; all other aspects are the same. Among them:
[0087] In Examples 1-3, PVDF was used for both the first and second adhesives, and PEG was used for both the third and fourth adhesives. The particle size of the first to fourth adhesives was adjusted, and the ratio K1 of the average particle size of the second adhesive to the average particle size of the first adhesive was kept at 2≤K1≤4, and the ratio K2 of the average particle size of the fourth adhesive to the average particle size of the third adhesive was kept at 2≤K2≤6.
[0088] In Examples 4-6, PVDF was used for both the first and second adhesives, and HPA was used for both the third and fourth adhesives. The average particle size of each adhesive was within its preferred range, and the ratios K1 and K2 met their respective preferred ranges.
[0089] In Examples 7-9, the first and second adhesives are both made of PTFE, and the third and fourth adhesives are both made of PEG. The average particle size of each adhesive is within its preferred range, and the ratios K1 and K2 satisfy their respective preferred ranges.
[0090] Comparative Examples 1-7
[0091] The adhesive compositions of Comparative Examples 1-7 are shown in Table 1, wherein:
[0092] The main difference between Comparative Examples 1-3 and Examples 1-9 lies in the particle size distribution of the adhesives; all other aspects are the same. In Comparative Examples 1-3, the average particle size of the first adhesive and the second adhesive are equal, as are the average particle sizes of the third and fourth adhesives. That is, the particle sizes of the adhesive particles in the first adhesive coating 101 corresponding to the positive electrode flat region 33 and the positive electrode thinning region 34 are identical, and the particle sizes of the adhesive particles in the second adhesive coating 102 corresponding to the negative electrode flat region 23 and the negative electrode thinning region 24 are identical. Furthermore, the particle size distribution and particle size ratios of the adhesives in Comparative Examples 1-3 are not within the preferred range.
[0093] In Comparative Example 4, although the particle size of each adhesive is within the preferred range, the particle size ratios K1 and K2 are not within the preferred range.
[0094] In Comparative Example 5, K1 and K2 are within the preferred range, but the particle sizes of the first to fourth adhesives are not within the preferred range.
[0095] In Comparative Example 6, the area of the first adhesive coating 101 corresponding to the positive electrode flat region 33 was not coated with adhesive, and the area of the second adhesive coating 102 corresponding to the negative electrode flat region 23 was not coated with adhesive. Adhesive was only coated in the areas corresponding to the positive electrode thinning region 34 and the negative electrode thinning region 24. That is, adhesive was only coated in the electrode thinning region corresponding to the separator.
[0096] Comparative Example 7 achieves thickness compensation for the electrode thinning area by increasing the thickness of the adhesive coating in the region corresponding to the electrode thinning area, and uses adhesive particles of a single size to form the adhesive coating. Specifically, in Comparative Example 7, thickness compensation is achieved by multiple coatings (i.e., increasing the coating thickness) in the second and fourth adhesive regions corresponding to the electrode thinning area, so that in the first adhesive coating 101, the thickness of the region coated with the second adhesive is greater than the thickness of the region coated with the first adhesive, and in the second adhesive coating 102, the thickness of the region coated with the fourth adhesive is greater than the thickness of the region coated with the third adhesive.
[0097] Table 1:
[0098]
[0099]
[0100] Effect Example
[0101] To better demonstrate that the battery cell prepared in the embodiments of the present invention has a stronger adhesion effect to the separator compared with conventional electrode sheets, the positive electrode thinning region 34 and the negative electrode thinning region 24 were tested as follows for Examples 1-9 and Comparative Examples 1-7:
[0102] (1) Separator-electrode peel strength test
[0103] The batteries prepared in Examples 1-9 and Comparative Examples 1-7 were discharged to a cutoff voltage of 2.8V, and then disassembled to obtain a separator / positive electrode bonding unit and a separator / negative electrode bonding unit. The bonding units were cut into 10mm wide strips. After the electrolyte on the surface of the bonding units evaporated, a universal tensile testing machine was used to perform a 180° peel tensile test on the separator and electrode. The tensile speed was 50mm / min, and the tensile stroke was 100mm. The force detected when the positive electrode (or negative electrode) peeled off was the peel strength. Thus, the adhesive strength values between the separator and the positive electrode (Table 2) and between the separator and the negative electrode (Table 3) were obtained. The adhesive strength value between the separator and the positive electrode includes the peel force between the separator and the thinned positive electrode region 34 and the peel force between the separator and the flat positive electrode region 33. The range between the two was calculated, as shown in Table 2. The bonding strength between the diaphragm and the negative electrode sheet includes the peel force between the diaphragm and the thinned area 24 of the negative electrode and the peel force between the diaphragm and the flat area 23 of the negative electrode. The range between the two is calculated, as shown in Table 3.
[0104] Table 2:
[0105]
[0106]
[0107] Table 3:
[0108]
[0109]
[0110] (2) Cell Cycle Capacity Retention Rate Test
[0111] The electrical performance of the prepared battery cells was evaluated by subjecting them to a 25°C cycle test and collecting cell capacity retention data. The specific test method was as follows: 1) Cell thermal equilibrium at 25°C; 2) 1C(A) constant current discharge to 2.0V; 3) Rest for 30 min; 4) 1C(A) CC to 2.8V, CV to 0.05C; 5) Rest for 30 min; 6) 1C(A) constant current discharge to 2.8V; 7) Repeat steps 3) to 6) for 2200 cycles or until the capacity retention rate is less than 80%. The capacity retention rate of the cycled battery cells was recorded, as shown in Table 4.
[0112] Table 4:
[0113]
[0114] (3) Electrode wrinkling test
[0115] To verify the effect of the battery cell prepared in this embodiment on improving the wrinkling of the negative electrode sheet, the prepared battery cell was disassembled under full capacity and the wrinkling ratio of the negative electrode sheet was counted. The results are shown in Table 5.
[0116] Table 5:
[0117]
[0118]
[0119] (4) Diaphragm air permeability test
[0120] The test was conducted using the Japanese Industrial Standard, which measures the time required for 100 mL of air to pass through a 1 square inch diaphragm at a pressure of 1.22 kPa. The results are shown in Table 6. In this embodiment, this time is referred to as the air permeability value, expressed in seconds (s). It can be understood that a higher air permeability value indicates poorer air permeability, and vice versa.
[0121] Table 6:
[0122]
[0123] According to Tables 1 and 2, the separators of Examples 1-9 used adhesives with different particle sizes in different areas of the adhesive coating. The particle size of the second adhesive was larger than that of the first adhesive, and the particle size of the fourth adhesive was larger than that of the third adhesive. This difference in adhesive particle size achieved thickness compensation in the electrode thinning area. In contrast, the separators of Comparative Examples 1-3 used adhesives with uniform particle size in the adhesive coating area. Based on the test results in Table 2, it can be seen that the difference in peel strength between the positive electrode thinning area 34 and the positive electrode flat area 33 in Examples 1-9 is smaller than that in Comparative Examples 1-3. The difference in peel strength between the positive electrode thinning area 34 and the positive electrode flat area 33 in Examples 1-9 is basically in the range of 0-0.3, while the difference in peel strength between Comparative Examples 1-3 is as high as 3.2. This indicates that the bonding consistency between the positive electrode and the separator is better in Examples 1-9.
[0124] The peel force data of the negative electrode sheet and the separator in Table 3 also show that the peel force difference between the separator and the thinned area and the flat area of the negative electrode sheet prepared in this embodiment is smaller, and the bonding consistency between the separator and the negative electrode sheet is also better than that of the single particle coating layer (Comparative Examples 1-3).
[0125] Although the particle sizes of the adhesives in Comparative Example 4 were within the preferred range, the particle size ratios K1 and K2 were not. As shown in Table 2, compared to Example 1, the difference in peel force between the flat and thinned electrode regions in Comparative Example 4 was larger. The peel force difference in Comparative Example 4 was 1.64 N / m, while the difference in peel force in Example 1 was 0.3 N / m. Referring to the cycling data in Table 4, Comparative Example 4 exhibited worse cycling performance than Example 1. The capacity retention rate after 500 cycles in Comparative Example 4 was 91.21%, while that in Example 1 was 93.21%. This is mainly due to the poor consistency of bonding effect in the cell region caused by the unreasonable particle size design of the diaphragm adhesive.
[0126] As can be seen from Table 4, the battery cells prepared in Examples 1, 5, and 9 have a capacity retention rate that is more than 1% higher than that prepared in Comparative Examples 1-3. For example, compared with Comparative Examples 1-3, Example 1 has a capacity retention rate that is 1% or higher higher after 500 cycles; Example 5 has a capacity retention rate that is 1% or higher higher after 500 cycles compared with Comparative Examples 2 and 3; and Example 9 has a capacity retention rate that is 1% or higher higher after 500 cycles compared with Comparative Examples 2 and 3.
[0127] Referring to Table 4, compared with Comparative Example 4 (diaphragm particle size within its preferred range, K1 and K2 ratio outside its preferred range) and Comparative Example 5 (diaphragm particle size outside its preferred range, K1 and K2 ratio within its preferred range), the cell prepared in Example 1 exhibits better capacity retention. As shown in Table 4, the 200cls cycle capacity retention of the cell prepared in Example 1 is approximately 2% higher than that of Comparative Examples 4 and 5, indicating that the cell prepared in this example has better electrical performance.
[0128] By comparing Comparative Example 5 with Examples 1-3, it can be seen that when the adhesive particle size is not within the preferred range (Comparative Example 5), the overall adhesion between the flat and thinned areas of the electrode and the separator is relatively low. Table 2 shows that the peel forces of the thinned positive electrode region 34 and the flat positive electrode region 33 in Comparative Example 5 are 0.75 N / m and 1.11 N / m, respectively, while the peel forces of the thinned positive electrode region 34 and the flat positive electrode region 33 in Examples 1-3 are above 4.66 N / m and 4.89 N / m, respectively. Table 3 shows that the peel forces of the thinned negative electrode region 24 and the flat negative electrode region 23 in Comparative Example 5 are 0.27 N / m and 0.31 N / m, respectively, while the peel forces of the thinned negative electrode region 24 and the flat negative electrode region 23 in Examples 1-3 are above 0.78 N / m and 0.95 N / m, respectively. The overall adhesion between the flat and thinned regions of the electrode sheet and the separator is relatively low. This will result in differences in the physical anchoring effect between the flat and thinned regions of the positive and negative electrode sheets and the separator, even when electrode cores are prepared under the same process parameters (hot pressing pressure, hot pressing temperature, hot pressing time, etc.). It is understandable that the flat and thinned regions of the electrode sheet have a certain degree of roughness, and the separator has different roughness due to the coating layers with different particle sizes. After hot pressing with certain parameters, the positive and negative electrode sheets will adhere together; this interaction between the electrode sheet and the separator constitutes physical anchoring. For separators with a separator adhesive particle size ratio and particle size composition within the preferred range, they have a stronger anchoring effect with the positive and negative electrode sheets. This stronger anchoring effect is mainly due to the better thickness compensation achieved by a reasonable particle size ratio design, thereby compensating for the thickness difference between the thinned and flat regions of the electrode sheet.
[0129] Furthermore, by combining Tables 2, 3, and 5, it can be found that the overall adhesion (peel strength of positive and negative electrodes) of the comparative examples is too low. The low adhesion leads to a generally high proportion of wrinkled electrode sheets in the cells. Among them, the proportion of wrinkled electrode sheets in the cells of comparative examples 4-7 exceeds 25%.
[0130] Compared with Examples 1-9, Comparative Example 6 only compensated for the thickness of the adhesive particle size in the thinned area. Although it can increase the peel strength of the thinned area to a certain extent, the flat area of the electrode corresponds to the uncoated diaphragm, which leads to a more serious problem of electrode wrinkling. As can be seen from Table 5, the wrinkling of the negative electrode is very serious, with a wrinkling rate as high as 87.5%. The severe wrinkling of the electrode also causes a certain degree of degradation in the cycle performance of the conductive core.
[0131] Furthermore, as can be seen from Table 4, the cycle capacity retention rate of the battery cell prepared in Comparative Example 6 is also lower than that of this embodiment (Examples 1, 5, and 9). It is speculated that this may be because the thinning area corresponding to the electrode is only coated with an adhesive layer, which leads to a more serious problem of electrode wrinkling. Electrode wrinkling often leads to electrode black spots and lithium plating, which is reflected in the lower cycle capacity retention rate of the battery cell in Comparative Example 6.
[0132] As can be seen from Table 5, the wrinkling rate of the battery cell electrode prepared in this embodiment is lower than that in the comparative embodiment. This is mainly because the negative electrode has a better adhesion to the separator, and the peeling force of the thinned area and flat area of the electrode is more consistent, which can effectively solve the problem of electrode wrinkling.
[0133] Comparative Example 7 compensates for the thickness of the electrode thinning area by increasing the thickness of the adhesive coating. While this method offers some benefit in ensuring consistency in the peel strength of the separator between the electrode thinning area and the normal area, it has some side effects compared to the thickness compensation methods in Examples 1-9, which utilize differences in adhesive particle size. Specifically, according to the separator permeability data in Table 6, Comparative Example 7's strategy results in a greater difference in permeability between the separator thinning area and the flat area compared to Example 1. In Comparative Example 7, the permeability value of the separator area corresponding to the electrode flat area is 155s, while the permeability value of the separator area corresponding to the electrode thinning area is 190s, a difference of 45s. Furthermore, the permeability value of the separator thinning area in Comparative Example 7 is significantly higher, leading to increased Li... + The transmission between the diaphragm and the electrode has a greater impedance, and the increase in impedance leads to an increase in electrode polarization.
[0134] Furthermore, based on the cell cycling data in Table 4, it can be seen that Comparative Example 7 also shows a certain degree of capacity decay compared to Example 1. In Example 1, the capacity retention rate after 200 cycles is 96.43%, and after 500 cycles it is 93.21%, while in Comparative Example 7 it is 94.11% after 200 cycles and after 500 cycles it is 90.77%. It is evident that the cycling performance of the cell in Comparative Example 7 is worse than that of the cell in this example. This may be due to the coating of multiple layers of separator adhesive on the thinned section of the separator, leading to increased permeability in the thinned section. This makes the separator more prone to pore blockage during cycling, resulting in lithium deposition at the cell interface and accelerated capacity decay.
[0135] While the present invention has been disclosed above, its scope of protection is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention, and all such changes and modifications will fall within the scope of protection of the present invention.
Claims
1. A method for preparing a diaphragm, characterized in that, include: Prepare the first slurry and the second slurry respectively; The first slurry and the second slurry are respectively coated on different areas of the base film (11) to form a flat area coating (12) and a thinned area coating (13). A diaphragm is obtained based on the base film (11), the flat area coating (12), and the thinned area coating (13); Wherein, the flat area coating (12) is made of a flat area adhesive, the thinned area coating (13) is made of a thinned area adhesive, and the average particle size of the flat area adhesive is smaller than the average particle size of the thinned area adhesive; The flat area adhesive includes a first adhesive and a third adhesive, and the thinned area adhesive includes a second adhesive and a fourth adhesive. The first adhesive and the second adhesive are disposed on the front side of the base film (11), and the average particle size of the first adhesive is smaller than the average particle size of the second adhesive. The third adhesive and the fourth adhesive are disposed on the back side of the base film (11), and the average particle size of the third adhesive is smaller than the average particle size of the fourth adhesive. The ratio of the average particle size of the second adhesive to the average particle size of the first adhesive is 2-4, and / or the ratio of the average particle size of the fourth adhesive to the average particle size of the third adhesive is 2-6. The first adhesive has an average particle size of 0.1-0.5 μm, the second adhesive has an average particle size of 1.0-2.0 μm; and / or, the third adhesive has an average particle size of 0.5-3.5 μm, and the fourth adhesive has an average particle size of 4.0-8.0 μm.
2. The method for preparing the diaphragm according to claim 1, characterized in that, The first adhesive includes polyvinylidene fluoride (PVDF) and polyvinylidene fluoride (PVDF). The second adhesive comprises one or more of hexafluoropropylene copolymer, polytetrafluoroethylene, copolymer derivatives of vinylidene fluoride, and copolymer derivatives of tetrafluoroethylene, wherein polyvinylidene fluoride is a copolymer of polyvinylidene fluoride and polyvinylidene fluoride. One or more of the following: hexafluoropropylene copolymers, polytetrafluoroethylene, copolymer derivatives of vinylidene fluoride, and copolymer derivatives of tetrafluoroethylene; and / or, The third adhesive includes one or more of polyethylene glycol, polymethyl acrylate, polymethyl methacrylate, polyethyl methacrylate, polybutyl methacrylate, polyacrylic acid, polyvinyl acetate, acrylate copolymers, styrene-butadiene latex, styrene-acrylic latex, polyvinyl alcohol, and sodium carboxymethyl cellulose. The fourth adhesive includes one or more of polyethylene glycol, polymethyl acrylate, polymethyl methacrylate, polyethyl methacrylate, polybutyl methacrylate, polyacrylic acid, polyvinyl acetate, acrylate copolymers, styrene-butadiene latex, styrene-acrylic latex, polyvinyl alcohol, and sodium carboxymethyl cellulose.
3. The method for preparing the diaphragm according to claim 1, characterized in that, Before coating the first slurry and the second slurry onto different regions of the base film (11), the method further includes coating the surface of the base film (11) with a ceramic slurry to obtain a ceramic coating (14).
4. A diaphragm, characterized in that, The membrane is prepared by the method described in any one of claims 1-3.
5. An electrode assembly, characterized in that, It includes a positive electrode (3), a negative electrode (2) and a diaphragm (1) as described in claim 4, wherein the diaphragm (1) is disposed between the positive electrode (3) and the negative electrode (2).
6. A secondary battery, characterized in that, Includes the electrode assembly as described in claim 5.
Citation Information
Patent Citations
Non-uniformly-glued diaphragm and battery with same
CN214153122U