Flame-retardant composites, methods of making and using the same

By controlling the pH value of the polymerization reaction, a flame-retardant composite material with uniform particle size and high sphericity was prepared, which solved the problem of inconsistent particle shape of flame-retardant capsules, improved the dispersibility of the battery and the ability to block thermal runaway reaction, and enhanced battery safety.

CN117960061BActive Publication Date: 2026-11-20JILIN UNIVERSITY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410166469.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-05
Publication Date
2026-11-20
Estimated Expiration
2044-02-05

AI Technical Summary

Technical Problem

The inconsistent shape of flame-retardant capsules in existing lithium-ion batteries leads to poor dispersion and uneven release, which cannot effectively block thermal runaway reactions and affects battery safety.

Method used

By controlling the pH value of the polymerization reaction between 8.5 and 10.0 and maintaining the pH fluctuation range ≤0.2, flame-retardant composite materials with uniform particle size and high sphericity are prepared, thereby achieving uniform coating of flame retardants on polymer monomers.

Benefits of technology

It improves the dispersibility and release consistency of flame-retardant composite materials in electrolytes, enabling timely and accurate blocking of thermal runaway reactions and enhancing battery safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117960061B_ABST
    Figure CN117960061B_ABST
Patent Text Reader

Abstract

The application provides a flame-retardant composite material and a preparation method and application thereof. The preparation method comprises the following steps: mixing a flame retardant and a polymer monomer in a solvent to prepare a reaction system, and performing a polymerization reaction on the reaction system under stirring, so that at least part of the flame retardant is coated in a polymer formed by the polymerization reaction; wherein from the start to the end of the polymerization reaction, the pH of the reaction system is controlled to be between 8.5 and 10.0 and the fluctuation range of the pH of the reaction system is controlled to be less than or equal to 0.2 by adding an alkaline adjusting agent. By controlling the pH of the polymerization reaction, the flame-retardant composite material with uniform particle size and high sphericity is obtained, and has the characteristics of good dispersibility and good release consistency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of battery technology, and in particular to a flame-retardant composite material, its preparation method, and its application. Background Technology

[0002] Lithium-ion batteries have become the mainstream power battery type due to their advantages such as high energy density, long cycle life, and low self-discharge rate. However, lithium-ion batteries still face some challenges in terms of energy density, cycle life, charging rate, and safety. In particular, with the continuous pursuit of higher energy density and ultra-fast charging technology, safety issues such as fire and explosion remain a thorny challenge.

[0003] In traditional technologies, the safety of automotive power batteries primarily relies on the Battery Management System (BMS), Thermal Management System, Fire Control and Extinguishing System, Safety Valves and Circuit Breakers, as well as the development of high-safety separators, electrode materials, and electrolytes. Among these, the use of flame retardants is an effective technical means for the safety protection of lithium-ion batteries, but it often comes at the cost of sacrificing battery electrochemical performance. Another advanced technology involves encapsulating flame retardants in capsules. When an abnormal situation occurs in the battery, these capsules rupture to release the flame retardant, offering advantages such as controlled release and reducing the negative impact of the flame retardant on battery electrochemical performance. However, the particle shape of existing flame-retardant capsules presents some problems, including poor dispersibility and uneven release. Summary of the Invention

[0004] Based on this, one embodiment of this application provides a flame-retardant composite material, its preparation method, and its application. By controlling the pH of the polymerization reaction, a flame-retardant composite material with uniform particle size and high sphericity is obtained, which has excellent dispersibility and release consistency.

[0005] In a first aspect, this application provides a method for preparing a flame-retardant composite material, the method comprising:

[0006] A reaction system is prepared by mixing a flame retardant and a polymer monomer in a solvent. The reaction system is then subjected to a polymerization reaction under stirring conditions, so that at least a portion of the flame retardant is encapsulated within the polymer formed by the polymerization reaction. From the start to the end of the polymerization reaction, the pH of the reaction system is controlled between 8.5 and 10.0 by adding an alkaline regulator, and the pH fluctuation range of the reaction system is controlled to be ≤0.2.

[0007] In some embodiments, the flame-retardant composite material that meets preset morphological and / or dimensional requirements is prepared by controlling at least one of the following conditions before or during the polymerization reaction:

[0008] (1) Control the amount of alkaline regulator added so that the initial pH of the reaction system reaches the preset pH requirement;

[0009] (2) During the polymerization reaction, the pH of the reaction system is maintained at the preset pH requirement by adding the alkaline regulator;

[0010] (3) The polymer monomer in the reaction system is introduced by multiple additions, and the coating state of the flame retardant is controlled by controlling the addition rate, the addition time interval and the amount added each time during the polymerization reaction.

[0011] In some embodiments, mixing the flame retardant, polymer monomer, and alkalinity modifier in a solvent includes:

[0012] A first solution and a second solution are prepared separately, wherein the first solution includes the flame retardant and the second solution includes the alkalinity regulator;

[0013] The first solution and the second solution are mixed evenly to obtain a mixture;

[0014] The polymer monomer is added to the mixture to prepare the reaction system;

[0015] Optionally, the solvent used in the first solution may include ethanol.

[0016] Optionally, the solvent used in the second solution may include deionized water.

[0017] In some embodiments, the mass ratio of the flame retardant to the polymer monomer is 1:(0.6~1.0).

[0018] In some embodiments, the polymerization reaction is carried out at a temperature of 15°C to 30°C, a stirring speed of 200 rpm to 1500 rpm, and a time of 12 h to 24 h.

[0019] In some embodiments, the reaction system is separated after the polymerization reaction is completed.

[0020] Optionally, the separation process includes centrifugation, washing, and drying performed sequentially.

[0021] In some embodiments, the centrifugation speed is 8000 rpm to 9000 rpm and the time is 2 min to 5 min.

[0022] In some embodiments, the drying temperature is 50°C to 70°C, and the drying time is 4 hours to 6 hours.

[0023] In some embodiments, the flame retardant includes at least one of phosphorus-based flame retardants, nitrogen-based flame retardants, halogen-based flame retardants, metal compound flame retardants, and electrolyte curing agents.

[0024] In some embodiments, the alkalinity regulator includes at least one of tris(hydroxymethyl)aminomethane, phosphate buffer, and bicarbonate buffer.

[0025] In some embodiments, the polymer monomer includes at least one of dopamine hydrochloride and methyl methacrylate; or the polymer monomer includes urea and acetaldehyde.

[0026] In a second aspect, this application provides a flame-retardant composite material, which includes a flame retardant and a polymer layer coated on the surface of the flame retardant; the flame-retardant composite material is prepared by the method for preparing flame-retardant composite materials as described in the first aspect.

[0027] In some embodiments, the average particle size of the flame-retardant composite material is 50 nm to 300 nm.

[0028] In some embodiments, the sphericity of the flame-retardant composite material is ≥0.8.

[0029] In some embodiments, the average thickness of the polymer layer is 10 nm to 50 nm.

[0030] In some embodiments, the particle size span of the flame-retardant composite material is ≤0.8, and the particle size span = (D90-D10) / D50, where D50 is the D50 particle size of the flame-retardant composite material, D10 is the D10 particle size of the flame-retardant composite material, and D90 is the D90 particle size of the flame-retardant composite material.

[0031] Thirdly, this application provides a battery comprising the flame-retardant composite material as described in the second aspect.

[0032] Compared with traditional technologies, this application has at least the following beneficial effects:

[0033] This application enables the uniform coating of polymer monomers with flame retardants by adjusting the pH during the preparation process of flame retardant composite materials. The resulting flame retardant composite materials have small and uniform particle size, high sphericity, better dispersibility in electrolyte, and can release flame retardants simultaneously during thermal runaway, effectively ensuring the timeliness of thermal runaway and improving battery safety. Attached Figure Description

[0034] Figure 1 This is an electron microscope image of the flame-retardant composite material prepared in Example 1 of this application.

[0035] Figure 2This is another electron microscope image of the flame-retardant composite material prepared in Example 1 of this application.

[0036] Figure 3 This is an electron microscope image of the flame-retardant composite material prepared in Comparative Example 1 of this application. Detailed Implementation

[0037] The present application will be further described in detail below with reference to the accompanying drawings, embodiments, and examples. These embodiments and examples are for illustrative purposes only and are not intended to limit the scope of the present application. The purpose of providing these embodiments and examples is to enable a more thorough and comprehensive understanding of the disclosure of the present application. It should also be understood that the present application can be implemented in many different forms and is not limited to the embodiments and examples described herein. Those skilled in the art can make various modifications or alterations without departing from the spirit of the present application, and the equivalent forms obtained also fall within the protection scope of the present application. Furthermore, numerous specific details are set forth in the following description to provide a fuller understanding of the present application. It should be understood that the present application can be implemented without one or more of these details.

[0038] In this application, "optionally," "optionally," and "optional" mean that something is optional, that is, it means that it is selected from either "with" or "without." If there are multiple "optional" entries in a technical solution, unless otherwise specified, and there are no contradictions or mutual constraints, each "optional" entry shall be independent.

[0039] In this application, the technical features described in an open-ended manner include both closed technical solutions consisting of the listed features and open technical solutions that include the listed features.

[0040] In this application, the terms "first," "second," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first," "second," etc., serve only as a non-exhaustive enumeration and should be understood as not constituting a closed limitation on quantity.

[0041] All references to this invention are incorporated herein by reference as if each document were individually incorporated by reference. Unless they conflict with the inventive purpose and / or technical solution of this application, the referenced documents involved in this invention are incorporated in their entirety and for all purposes. When references are made in this invention, the definitions of relevant technical features, terms, nouns, phrases, etc., are also incorporated herein by reference. When references are made in this invention, examples and preferred embodiments of the relevant technical features cited may also be incorporated herein by reference, but only to the extent that they enable the implementation of this invention. It should be understood that when the cited content conflicts with the description in this application, this application shall prevail or modifications shall be made adaptively based on the description in this application.

[0042] In traditional technologies, flame retardant capsules are prepared by encapsulating flame retardants within a capsule shell using methods such as solution processing, emulsification, and spray drying. However, the resulting flame retardant capsules exhibit inconsistent sizes and poor sphericity, leading to poor dispersibility when added to the electrolyte. Furthermore, although the same capsule shell is used for encapsulation, the inconsistent size of each capsule results in different release conditions, failing to promptly and accurately block thermal runaway reactions. This application, by controlling the pH during the preparation process, yields a flame retardant composite material with small, uniform particle size and good sphericity. This material not only exhibits good dispersibility in the electrolyte but also demonstrates consistent flame retardant release during thermal runaway, enabling timely and accurate blocking of thermal runaway reactions and improving battery safety.

[0043] The first aspect of this application provides a method for preparing a flame-retardant composite material, the method comprising:

[0044] A reaction system is prepared by mixing a flame retardant and a polymer monomer in a solvent. The reaction system is then subjected to a polymerization reaction under stirring conditions, so that at least a portion of the flame retardant is encapsulated within the polymer formed by the polymerization reaction. From the start to the end of the polymerization reaction, the pH of the reaction system is controlled between 8.5 and 10.0 by adding an alkaline regulator, and the pH fluctuation range of the reaction system is controlled to be ≤0.2.

[0045] This application enables the uniform coating of polymer monomers with flame retardants by adjusting the pH during the preparation process of flame retardant composite materials. The resulting flame retardant composite materials have small and uniform particle size, high sphericity, better dispersibility in electrolyte, and can release flame retardants simultaneously during thermal runaway, effectively ensuring the timeliness of thermal runaway and improving battery safety.

[0046] The pH of the polymerization reaction can be 8.5, 8.6, 8.7, 8.8, 8.9, 9.0, 9.1, 9.2, 9.3, 9.4, 9.5, 9.6, 9.7, 9.8, 9.9 or 10.0.

[0047] This application controls the pH of the polymerization reaction to prepare particles with uniform particle size and high sphericity. If the pH is relatively low, the resulting spherical microcapsule particles may be larger; if the pH is relatively high, the resulting microcapsule spherical particles may be smaller, or even form a black amorphous polymer material instead of particles.

[0048] It is understood that the flame retardant in this application can be a material that prevents the battery from undergoing a combustion reaction, or a material that can block the combustion of the battery after it has started to burn, thereby achieving the purpose of extinguishing the fire. The flame retardant mechanism can be endothermic, covering, chain reaction inhibition, and asphyxiation by non-flammable gases. The endothermic effect of the flame retardant refers to its ability to absorb heat generated during the thermal runaway and combustion reaction stages in a short time, thereby preventing and controlling the further occurrence of the heat generation and combustion reactions. The covering effect of the flame retardant refers to its ability to form a barrier layer at thermal runaway temperatures, isolating the battery active materials from oxygen, providing heat insulation, oxygen isolation, and preventing the escape of flammable gases, thus achieving the flame retardant purpose. The chain reaction inhibition effect of the flame retardant refers to its ability to capture free radicals during the reaction process during the thermal runaway and combustion stages, thereby interfering with the heat generation and combustion reactions. For example, the flame retardant can react with the active materials or solidify the electrolyte, thereby preventing the heat generation reaction from proceeding. The asphyxiation effect of flame retardants on non-flammable gases refers to the fact that when flame retardants are heated, they decompose into non-flammable gases, diluting the concentration of flammable gases released from the combustible material to below the lower flammability limit. At the same time, they also dilute the oxygen concentration in the combustion zone, preventing the continuation of combustion and thus achieving the effect of flame retardancy.

[0049] In some embodiments, before or during the polymerization reaction, the amount of alkaline regulator added is controlled to bring the initial pH of the reaction system to a preset pH requirement, thereby preparing the flame-retardant composite material that meets preset morphological and / or size requirements.

[0050] In some embodiments, the flame-retardant composite material that meets preset morphological and / or size requirements is prepared by adding the alkaline regulator to maintain the pH of the reaction system at a preset pH requirement before or during the polymerization reaction.

[0051] In some embodiments, the polymer monomers in the reaction system are introduced in multiple additions before or during the polymerization reaction, and the coating state of the flame retardant is controlled by controlling the addition rate, the addition time interval, and the amount added each time during the polymerization reaction.

[0052] This application controls the coating state of the flame retardant by controlling the addition rate, addition time interval and amount of polymer monomers, so as to prepare the flame retardant composite material that meets the preset morphology and / or preset size requirements.

[0053] In some embodiments, mixing the flame retardant, polymer monomer, and alkalinity modifier in a solvent includes:

[0054] A first solution and a second solution are prepared separately, wherein the first solution includes the flame retardant and the second solution includes the alkalinity regulator;

[0055] The first solution and the second solution are mixed evenly to obtain a mixture;

[0056] The polymer monomer is added to the mixture to prepare the reaction system.

[0057] Optionally, the solvent used in the first solution may include ethanol.

[0058] Optionally, the solvent used in the second solution may include deionized water.

[0059] In some embodiments, the mass ratio of the flame retardant to the polymer monomer is 1:(0.6~1.0), for example, it can be 1:0.60, 1:0.64, 1:0.68, 1:0.72, 1:0.76, 1:0.80, 1:0.84, 1:0.88, 1:0.92, 1:0.96 or 1:1.00.

[0060] In some embodiments, the temperature of the polymerization reaction is 15°C to 30°C, for example, it can be 15°C, 16°C, 17°C, 18°C, 19°C, 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C or 30°C.

[0061] This application controls the temperature of the polymerization reaction to ensure that the resulting flame-retardant composite material has small and uniform particle size and high sphericity. If the polymerization reaction temperature is relatively low, the microcapsule particles may be large. If the polymerization reaction temperature is relatively high, the particles may be small, or even a black amorphous polymer material may be formed instead of particles.

[0062] In some embodiments, the stirring speed of the polymerization reaction is 200 rpm to 1500 rpm, for example, 200 rpm, 300 rpm, 400 rpm, 500 rpm, 600 rpm, 700 rpm, 800 rpm, 900 rpm, 1000 rpm, 1100 rpm, 1200 rpm, 1300 rpm, 1400 rpm, or 1500 rpm.

[0063] In some embodiments, the polymerization reaction time is 12h to 24h, for example, it can be 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h or 24h.

[0064] In some embodiments, the reaction system is separated after the polymerization reaction is completed.

[0065] Optionally, the separation process includes centrifugation, washing, and drying performed sequentially.

[0066] In some embodiments, the cleaning includes at least one of water washing and organic solvent cleaning. For example, ethanol is used as the organic solvent.

[0067] Optionally, the cleaning includes sequential deionized water washing and organic solvent washing.

[0068] In some embodiments, the centrifugation speed is 8000 rpm to 9000 rpm, for example, it can be 8000 rpm, 8100 rpm, 8200 rpm, 8300 rpm, 8400 rpm, 8500 rpm, 8600 rpm, 8700 rpm, 8800 rpm, 8900 rpm or 9000 rpm.

[0069] In some embodiments, the centrifugation time is 2 min to 5 min, for example, it can be 2.0 min, 2.3 min, 2.6 min, 2.9 min, 3.2 min, 3.5 min, 3.8 min, 4.1 min, 4.4 min, 4.7 min or 5.0 min.

[0070] In some embodiments, the drying temperature is 50°C to 70°C, for example, it can be 50°C, 52°C, 54°C, 56°C, 58°C, 60°C, 62°C, 64°C, 66°C, 68°C or 70°C.

[0071] In some embodiments, the drying time is 4h to 6h, for example, it can be 4.0h, 4.2h, 4.4h, 4.6h, 4.8h, 5.0h, 5.2h, 5.4h, 5.6h, 5.8h or 6.0h.

[0072] In some embodiments, the flame retardant may be an inorganic flame retardant or an organic flame retardant.

[0073] In some embodiments, the flame retardant includes at least one of phosphorus-based flame retardants, nitrogen-based flame retardants, halogen-based flame retardants, metal compound flame retardants, and electrolyte curing agents;

[0074] In some embodiments, the phosphorus-based flame retardant refers to a flame retardant containing phosphorus, such as triphenyl phosphate, tricresyl phosphate, or tri(xyl) phosphate. Phosphorus-based flame retardants react at high temperatures to produce phosphorus compounds, forming a gas barrier layer and a char layer, thereby preventing the combustion reaction and achieving a flame-retardant effect.

[0075] The nitrogen-based flame retardant refers to a flame retardant containing nitrogen, such as melamine, melamine cyanuric acid, etc. Nitrogen-based flame retardants decompose at high temperatures to release non-flammable gases such as CO2, NO2, N2, NH3, and H2O, which can dilute flammable gases, cover and surround the polymer, and isolate the polymer from oxygen in the air. At the same time, nitrogen can capture high-energy free radicals and inhibit the continuous combustion of the polymer, thereby achieving the purpose of flame retardancy.

[0076] The halogenated flame retardant refers to a flame retardant containing halogen elements such as fluorine, chlorine, and bromine. Examples include brominated polystyrene, polydibromostyrene, brominated epoxy high-molecular-weight flame retardants, tetrabromobisphenol A carbonate oligomers, polydibromophenyl ether, and polypentabromophenyl acrylate. Halogenated flame retardants decompose at high temperatures to produce halogen compounds, which inhibit the combustion chain reaction and form a gas barrier layer, thereby achieving a flame-retardant effect.

[0077] The metal compound flame retardant includes at least one of magnesium-based flame retardants (magnesium hydroxide), antimony-based flame retardants (antimony oxide, sodium antimonate), aluminum hydroxide, zinc borate, molybdenum oxide, and ammonium molybdate.

[0078] The electrolyte curing agent refers to an agent that can interact with the electrolyte to control its dielectric constant or viscosity, aiming to suppress Joule heating by forcibly increasing internal resistance by disrupting ionic conductivity. The curing agent can increase the viscosity of the electrolyte, transforming the liquid electrolyte into a non-conductive solid or gel-like substance. Optionally, the electrolyte curing agent includes one or more of glycol and amine compounds. For example, amine curing agents include, but are not limited to: 1,3-propanediamine, benzylamine, dibenzylamine (DBA), 1,2-ethylenediamine (1,2-EDA), and trihexylamine (THA); glycol curing agents include, but are not limited to: 1,2-ethylenediol, 1,3-propanediol, and 1,5-pentanediol.

[0079] In some embodiments, the alkalinity regulator includes at least one of tris(hydroxymethyl)aminomethane, phosphate buffer, and bicarbonate buffer. Tris(hydroxymethyl)aminomethane is preferred.

[0080] This application uses tris(hydroxymethyl)aminomethane as an alkaline regulator. This flame retardant is weakly alkaline and suitable for precise adjustment of the solution pH value within a small range. In addition, a tris(hydroxymethyl)aminomethane buffer solution is used. The average size of the polydopamine spherical particles is smaller and the particle size is more uniform than that in phosphate and bicarbonate buffer solutions.

[0081] In some embodiments, the polymer monomer includes at least one of dopamine hydrochloride and methyl methacrylate; or the polymer monomer includes urea and acetaldehyde.

[0082] The second aspect of this application provides a flame-retardant composite material, which includes a flame retardant and a polymer layer coated on the surface of the flame retardant; the flame-retardant composite material is prepared by the method for preparing flame-retardant composite materials as described in the first aspect.

[0083] In some embodiments, the average particle size of the flame-retardant composite material is 50nm~300nm, for example, it can be 50nm, 60nm, 80nm, 100nm, 120nm, 140nm, 160nm, 180nm, 200nm, 220nm, 240nm, 260nm, 280nm or 300nm.

[0084] In some embodiments, the sphericity of the flame-retardant composite material is ≥0.8, for example, it can be 0.80, 0.81, 0.82, 0.83, 0.84, 0.85, 0.86, 0.87, 0.88, 0.89, 0.90, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99 or 1.00.

[0085] The flame-retardant composite material prepared in this application has a small particle size, a sphericity ≥0.8, and a particle appearance close to spherical. It has good dispersibility in the electrolyte and can quickly and uniformly release the flame retardant when the battery experiences thermal runaway, thus inhibiting the occurrence of battery thermal runaway.

[0086] In some embodiments, the average thickness of the polymer layer is 10nm to 50nm, for example, it can be 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm or 50nm.

[0087] In some embodiments, the particle size span of the flame-retardant composite material is ≤0.8, for example, it can be 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2 or 0.1, and the particle size span = (D90-D10) / D50, where D50 is the D50 particle size of the flame-retardant composite material, D10 is the D10 particle size of the flame-retardant composite material, and D90 is the D90 particle size of the flame-retardant composite material.

[0088] The flame-retardant composite material prepared in this application has a particle size range of ≤0.8 and the particle size of the flame-retardant composite material is close, that is, the particle size of each flame-retardant composite material is basically the same. Therefore, in the event of thermal runaway, the flame-retardant composite material can release flame retardants at the same temperature, thereby accurately and timely blocking the thermal runaway reaction.

[0089] It should be noted that the particle size span represents the range of particle size distribution of the material. The smaller the particle size span, the narrower the particle size distribution range, and the closer the particle size of each particle is to the D50 particle size.

[0090] A third aspect of this application provides a battery comprising a flame-retardant composite material as described in the second aspect.

[0091] In some embodiments, the battery includes a casing filled with electrolyte, and a battery cell immersed in electrolyte is disposed inside the casing. The battery cell includes a positive electrode and a negative electrode stacked together, and a separator is disposed between the positive electrode and the negative electrode. The electrolyte includes the flame-retardant composite material.

[0092] In some embodiments, the flame-retardant composite material accounts for 3% to 15% of the mass of the electrolyte, for example, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15%.

[0093] The embodiments of the present invention will be described in detail below with reference to examples. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. For experimental methods in the following embodiments where specific conditions are not specified, please refer to the guidelines given in this invention, or follow experimental manuals or conventional conditions in the art, or follow the conditions recommended by the manufacturer, or refer to experimental methods known in the art.

[0094] The average particle size was obtained through image shadow statistics using transmission electron microscopy. The average thickness was calculated by averaging the maximum and minimum thicknesses of the shell obtained using transmission electron microscopy.

[0095] Example 1

[0096] Weigh 0.5g of triphenyl phosphate and dissolve it in 20mL of anhydrous ethanol. Sonicate for 10 minutes to disperse it evenly to obtain a flame retardant solution.

[0097] Weigh 0.605g of tris(hydroxymethyl)aminomethane and dissolve it in 500mL of deionized water. Stir for 10 minutes to disperse it evenly to obtain an alkaline regulator solution.

[0098] The flame retardant solution was stirred and added to the alkaline regulator solution, and after being dispersed evenly, the first solution was obtained.

[0099] 0.4 g of dopamine hydrochloride was added to the first solution, and the polymerization reaction was carried out at 25 °C and pH 9 under stirring for 24 h. During the polymerization reaction, tris(hydroxymethyl)aminomethane was added to maintain the pH of the polymerization reaction at 9.

[0100] The solution after polymerization was centrifuged at 8600 rpm for 3 min, washed three times with deionized water and once with ethanol, and then vacuum dried at 60 °C for 5 h to obtain a flame-retardant composite material of polydopamine-coated triphenyl phosphate. Figure 1 and Figure 2 As shown, the average particle size of the flame-retardant composite material is 182 nm.

[0101] Example 2

[0102] Weigh 0.5g of triphenyl phosphate and dissolve it in 20mL of anhydrous ethanol. Sonicate for 10 minutes to disperse it evenly to obtain a flame retardant solution.

[0103] Weigh 0.605g of tris(hydroxymethyl)aminomethane and dissolve it in 500mL of deionized water. Stir for 10 minutes to disperse it evenly to obtain an alkaline regulator solution.

[0104] The flame retardant solution was stirred and added to the alkaline regulator solution, and after being dispersed evenly, the first solution was obtained.

[0105] 0.5 g of dopamine hydrochloride was added to the first solution, and the polymerization reaction was carried out at 25 °C and pH 8.5 under stirring for 24 h. During the polymerization reaction, tris(hydroxymethyl)aminomethane was added to maintain the pH of the polymerization reaction at 8.5.

[0106] The solution after polymerization was centrifuged at 8000 rpm for 5 min, washed three times with deionized water and once with ethanol, and then vacuum dried at 70 °C for 4 h to obtain a flame-retardant composite material of polydopamine-coated triphenyl phosphate with an average particle size of 212 nm.

[0107] Example 3

[0108] Weigh 0.5g of triphenyl phosphate and dissolve it in 20mL of anhydrous ethanol. Sonicate for 10 minutes to disperse it evenly to obtain a flame retardant solution.

[0109] Weigh 0.605g of tris(hydroxymethyl)aminomethane and dissolve it in 500mL of deionized water. Stir for 10 minutes to disperse it evenly to obtain an alkaline regulator solution.

[0110] The flame retardant solution was stirred and added to the alkaline regulator solution, and after being dispersed evenly, the first solution was obtained.

[0111] Add 0.5g of dopamine hydrochloride to the first solution and carry out the polymerization reaction at 25°C and pH 10 with stirring for 24h. During the polymerization reaction, tris(hydroxymethyl)aminomethane is added to maintain the pH of the polymerization reaction at 10.

[0112] The solution after polymerization was centrifuged at 9000 rpm for 2 min, washed three times with deionized water and once with ethanol, and then vacuum dried at 50 °C for 6 h to obtain a flame-retardant composite material of polydopamine-coated triphenyl phosphate with an average particle size of 53 nm.

[0113] Example 4

[0114] The flame-retardant composite material was prepared according to the method of Example 1, except that the polymerization temperature was 10°C.

[0115] Example 5

[0116] The flame-retardant composite material was prepared according to the method of Example 1, except that the polymerization temperature was 35°C.

[0117] Comparative Example 1

[0118] The flame-retardant composite material was prepared according to the method of Example 1, the only difference being that no alkaline regulator was added during the polymerization reaction to maintain the pH. The resulting flame-retardant composite material was as follows: Figure 3 As shown.

[0119] Comparative Example 2

[0120] The flame-retardant composite material was prepared according to the method of Example 1, except that the pH was maintained at 7.5 during the polymerization reaction.

[0121] Comparative Example 3

[0122] The flame-retardant composite material was prepared according to the method of Example 1, except that the pH was maintained at 11 during the polymerization reaction.

[0123] The flame-retardant composite materials prepared in the above embodiments and comparative examples were added to the electrolyte for testing. The testing methods included:

[0124] 10% of the flame-retardant composite material was added to an electrolyte of type KLD-LP11 (solute: 1.2 mol / L LiPF6; solvent: EC:EMC volume ratio: 3:7), and the self-extinguishing time and conductivity of the electrolyte of the battery were tested.

[0125] The method for testing the self-extinguishing time of the electrolyte involves placing approximately 0.5 grams of electrolyte into a petri dish with a diameter of 7 cm. The electrolyte is then exposed to the flame of a burner for 3 seconds. If ignition occurs, the time from when the burner is removed (after 3 seconds) until the flame is completely extinguished is recorded, and the ratio of burning time to mass is denoted as SET.

[0126] The electrolyte conductivity was tested using a Consort K912 conductivity meter with an SK21T microelectrode probe, conducted in an argon-filled glove box. The conductivity meter was calibrated outside the glove box using a KCl standard solution. At room temperature, 4 mL of electrolyte sample was placed in a 10 mL centrifuge tube. The electrode probe was then inserted into the electrolyte in the centrifuge tube, ensuring the electrolyte submerged at least 1 / 3 of the probe tip. The conductivity value was read after the reading stabilized. The test results are shown in Table 1.

[0127] Table 1

[0128]

[0129] As can be seen from the table above:

[0130] (1) Compared with Examples 4-5, Example 1 shows that the present application controls the temperature of the polymerization reaction, thereby producing microcapsules with more uniform size and better sphericity. Microcapsules with more uniform morphology can improve the safety performance and conductivity of the electrolyte when added to the electrolyte. If the temperature of the polymerization reaction is relatively low, the microcapsule formation may be slower or it may be difficult to form microcapsules with spherical structure. If the temperature of the polymerization reaction is relatively high, the microcapsule may form rapidly, resulting in a wide range of particle sizes and uneven microcapsule morphology.

[0131] (2) Compared with Comparative Example 1, Example 1 combines Figure 1-3 It can be seen that the flame-retardant composite material prepared in this application has good particle size uniformity, small particle size and high sphericity; while the particles prepared in Comparative Example 1 have uneven particle size, with large and small particles, and the particles in Comparative Example 1 have poor sphericity, with defects such as protrusions or depressions on the surface of the particles, which causes the particles to break in advance at the defective structures during the thermal runaway process, and cannot accurately and timely block the thermal runaway reaction.

[0132] (3) Compared with Comparative Examples 2-3, Example 1 shows that the present application controls the pH of the polymerization reaction to prepare particles with consistent particle size and high sphericity. If the pH is relatively low, it may result in a large range of microcapsule size and particle size; if the pH is relatively high, the microcapsule size may be small and the particle size range may be large.

[0133] Through the above examples and comparative examples, it can be seen that by adjusting the pH during the preparation process of flame-retardant composite materials, this application can achieve uniform coating of polymer monomers with flame retardants. The resulting flame-retardant composite materials have small particle size and uniform particle size, high sphericity, better dispersibility in electrolyte, and can release flame retardants simultaneously during thermal runaway, effectively ensuring the timeliness of thermal runaway and improving battery safety.

[0134] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0135] The above embodiments merely illustrate several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.

Claims

1. A method for preparing a flame-retardant composite material, characterized in that, The preparation method includes: A reaction system is prepared by mixing a flame retardant and a polymer monomer in a solvent. The reaction system is then subjected to a polymerization reaction under stirring conditions, so that at least a portion of the flame retardant is encapsulated within the polymer formed by the polymerization reaction. From the start to the end of the polymerization reaction, the pH of the reaction system is controlled between 8.5 and 10.0 by adding an alkaline regulator, and the pH fluctuation range of the reaction system is controlled to be ≤0.

2. The temperature of the polymerization reaction is 15℃ to 30℃. The mass ratio of the flame retardant to the polymer monomer is 1:(0.6~1.0); the flame retardant includes at least one of phosphorus-based flame retardants, nitrogen-based flame retardants, halogen-based flame retardants, metal compound flame retardants, and electrolyte curing agents; the alkalinity regulator includes at least one of tris(hydroxymethyl)aminomethane, phosphate buffer, and bicarbonate buffer; the polymer monomer includes at least one of dopamine hydrochloride and methyl methacrylate; or the polymer monomer includes urea and acetaldehyde.

2. The method for preparing the flame-retardant composite material as described in claim 1, characterized in that, Before or during the polymerization reaction, the flame-retardant composite material that meets the preset morphology and / or preset size requirements is prepared by controlling at least one of the following conditions: (1) Control the amount of alkaline regulator added so that the initial pH of the reaction system reaches the preset pH requirement; (2) During the polymerization reaction, the pH of the reaction system is maintained at the preset pH requirement by adding the alkaline regulator; (3) The polymer monomer in the reaction system is introduced by multiple additions, and the coating state of the flame retardant is controlled by controlling the addition rate, the addition time interval and the amount added each time during the polymerization reaction.

3. The preparation method according to claim 1, characterized in that, The step of mixing the flame retardant, polymer monomer, and alkaline modifier in a solvent includes: A first solution and a second solution are prepared separately, wherein the first solution includes the flame retardant and the second solution includes the alkalinity regulator; The first solution and the second solution are mixed evenly to obtain a mixture; The polymer monomer is added to the mixture to prepare the reaction system.

4. The preparation method according to claim 3, characterized in that, The solvent used in the first solution includes ethanol.

5. The preparation method according to claim 3, characterized in that, The solvent used in the second solution includes deionized water.

6. The preparation method according to claim 1, characterized in that, The polymerization reaction is carried out at a stirring speed of 200 rpm to 1500 rpm for a duration of 12 h to 24 h.

7. The preparation method according to any one of claims 1-4, characterized in that, After the polymerization reaction is completed, the reaction system is separated.

8. The preparation method according to claim 7, characterized in that, The separation process includes centrifugation, washing, and drying performed sequentially.

9. The preparation method according to claim 8, characterized in that, The separation process satisfies at least one of the following conditions: (1) The centrifugation speed is 8000 rpm to 9000 rpm and the time is 2 min to 5 min; (2) The drying temperature is 50℃~70℃ and the time is 4h~6h.

10. A flame-retardant composite material, characterized in that, The flame-retardant composite material includes a flame retardant and a polymer layer coated on the surface of the flame retardant; The flame-retardant composite material is prepared by the method described in any one of claims 1-9.

11. The flame-retardant composite material as described in claim 10, characterized in that, The flame-retardant composite material satisfies at least one of the following conditions: (1) The average particle size of the flame-retardant composite material is 50 nm to 300 nm; (2) The sphericity of the flame-retardant composite material is ≥0.8; (3) The average thickness of the polymer layer is 10 nm to 50 nm; (4) The particle size span of the flame-retardant composite material is ≤0.8, and the particle size span is (D90-D10) / D50, where D50 is the D50 particle size of the flame-retardant composite material, D10 is the D10 particle size of the flame-retardant composite material, and D90 is the D90 particle size of the flame-retardant composite material.

12. A battery, characterized in that, The battery comprises the flame-retardant composite material as described in claim 10 or 11.

Citation Information

Patent Citations

  • Spherical phosphor nitrogen synergistic fire retardant and preparation method thereof

    CN108559041A