A flotation collector and its application in low-grade spodumene
By using a collector containing soluble inorganic base, fatty acid, hydroxamic acid, polyoxyethylene polyoxypropylene ether block copolymer and Tween-like surfactants, the problem of poor selectivity in low-grade spodumene ore was solved, achieving efficient flotation and stable resource utilization.
Patent Information
- Application Number
- CN202410073947.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-18
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-01-18
AI Technical Summary
Traditional reagent systems have poor selectivity when processing low-grade spodumene ore, resulting in high reagent consumption, low concentrate grade and low recovery rate, making it difficult to meet the requirements for the development and utilization of low-grade spodumene resources.
A flotation collector containing soluble inorganic base, fatty acid, hydroxamic acid, polyoxyethylene polyoxypropylene ether block copolymer and Tween surfactant is used. Through saponification, chelation, defoaming and emulsification, the selectivity and stability of the collector are improved, the flotation process is simplified, the floating of slime is suppressed and the flotation efficiency is improved.
It significantly improved the grade and recovery rate of low-grade spodumene flotation concentrate, reduced reagent consumption, improved the stability and efficiency of the flotation process, and achieved efficient resource utilization.
Smart Images

Figure CN117960394B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a flotation collector and its application in low-grade spodumene, belonging to the field of mineral flotation technology. Background Technology
[0002] Lithium is a crucial metal widely used in battery technology, alloy preparation, pharmaceutical production, the glass industry, and the nuclear industry. With the rapid rise of electric vehicles and renewable energy, market demand for lithium has increased dramatically. As one of the main natural lithium-extraction minerals, spodumene faces new challenges in its mining and processing due to this surge in market demand.
[0003] my country is rich in spodumene resources, but many are associated deposits with relatively low grades, making processing difficult. These ores have low lithium content, complex composition, and are prone to mud formation. Flotation is the most common and effective method for processing this type of spodumene. However, the traditional "three alkalis and two soaps" reagent system (modifiers sodium carbonate, sodium hydroxide, and sodium sulfide; collectors oxidized paraffin soap and naphthenic acid soap) cannot meet the processing requirements of these ores, resulting in poor selectivity and unstable production. Low-grade spodumene ores contain many impurities, especially aluminosilicate minerals such as feldspar, quartz, chlorite, and amphibole, which have similar surface properties to spodumene and are prone to mud formation. Under traditional reagent systems, they easily float, further exposing the disadvantage of insufficient reagent selectivity. Ultimately, this leads to high reagent consumption, low concentrate grade, and low recovery rate, severely limiting the development and utilization of low-grade spodumene resources.
[0004] Therefore, improving the selectivity of collectors while maintaining their collecting capacity is key to processing low-grade spodumene ore. Developing a highly efficient collector and flotation process suitable for low-grade spodumene flotation is of great significance for improving resource utilization and ensuring resource reserves.
[0005] In view of this, the present invention is hereby proposed. Summary of the Invention
[0006] To address the problems of high reagent consumption, low concentrate recovery rate, low grade, and unstable production in the flotation of low-grade spodumene ore, the first objective of this invention is to provide a flotation collector with good dispersibility and both collecting capacity and selectivity. This collector can not only serve as a highly efficient collector for high-quality spodumene ore, but also significantly improve the flotation performance of low-grade spodumene.
[0007] The second objective of this invention is to provide an application of a flotation collector for the flotation process of low-grade spodumene, which eliminates the need for desliming and can ensure flotation indicators such as grade and recovery rate of spodumene while greatly simplifying the flotation process.
[0008] To achieve the above-mentioned technical objectives, the present invention provides a flotation collector, which is obtained by reacting raw materials including a soluble inorganic base, fatty acid, hydroxamic acid, polyoxyethylene polyoxypropylene ether block copolymer and Tween surfactant.
[0009] The collector of this invention uses fatty acids as its main component. After partial saponification of the fatty acids by a soluble inorganic alkali, a mixture of fatty acids and sodium fatty acids is obtained, ensuring the recovery rate of spodumene in flotation. The key to this collector lies in the addition of hydroxamic acid, polyoxyethylene-polyoxypropylene ether block copolymer, and Tween-like surfactants, in addition to specific amounts of soluble inorganic alkali and fatty acids. Hydroxamic acid, as an auxiliary collector, can chelate with metal ions to form stable chelates, and this chelation effect has high selectivity, compensating for the poor selectivity of fatty acids. The polyoxyethylene-polyoxypropylene ether block copolymer is a type of nonionic surfactant with excellent defoaming ability. The role of the Tween-like surfactant is to fully emulsify and disperse the components of the collector, forming a homogeneous state and enhancing the stability of the collector. Low-grade spodumene typically has a high mud content, requiring desliming in existing technologies. The flotation collector provided in this invention, without desliming, can suppress the indiscriminate flotation of fine-grained slime, improving the viscosity and poor flowability of flotation foam, and enhancing flotation efficiency and process stability. Tween-type surfactants can adjust the foam structure and improve dispersibility. In summary, fatty acid components improve flotation recovery, hydroxamic acid components adjust concentrate grade, polyoxyethylene-polyoxypropylene ether block copolymers adjust foam state, Tween improves collector stability, and the synergistic effects of saponification, foaming, defoaming, and emulsification among the components result in a collector with excellent collecting ability and selectivity.
[0010] As a preferred embodiment, the flotation collector is obtained by reacting the following raw materials in parts by weight: 7-30 parts soluble inorganic alkali, 50-70 parts fatty acid, 5-15 parts hydroxamic acid, 2-10 parts polyoxyethylene-polyoxypropylene ether block copolymer, 5-20 parts Tween surfactant, and 60-100 parts water. A higher or lower proportion of components such as fatty acid, hydroxamic acid, polyoxyethylene-polyoxypropylene ether block copolymer, and Tween surfactant in the flotation collector will affect the collection effect of the collector in different ways.
[0011] As a preferred embodiment, the soluble inorganic base is a commonly used soluble inorganic base, such as sodium hydroxide, sodium carbonate, or potassium hydroxide.
[0012] As a preferred embodiment, the fatty acid includes at least one long-chain fatty acid with a carbon chain length greater than 12, and industrial products mainly composed of the above-mentioned fatty acids can also be used in this invention. More preferably, oleic acid and / or soybean oleic acid are used.
[0013] As a preferred embodiment, the hydroxamic acid is at least one selected from alkyl hydroxamic acids, salicylic acid, benzoic acid, naphtholic acid, and amide hydroxamic acids, with a carbon chain length greater than 4. More preferably, the hydroxamic acid is at least one selected from C7-C9 alkyl hydroxamic acids and benzoic acid.
[0014] As a preferred embodiment, the polyoxyethylene polyoxypropylene ether block copolymer is at least one selected from the Pluronic series L31, L35, L42, L43, L44, L45, L61, L62, L63, L64, P65, P84, F38, and F68. The molecular formula of the polyoxyethylene polyoxypropylene ether block copolymer is HO(C2H4O)a(C3H6O)b(C2H4O)cH. As a further preferred embodiment, the polyoxyethylene polyoxypropylene ether block copolymer is L61 or L64.
[0015] As a preferred embodiment, the Tween surfactant is selected from at least one of Tween 20, Tween 21, Tween 40, Tween 60, Tween 61, Tween 80, Tween 81, and Tween 85, or an industrial product with the above substances as its main components. The Tween surfactants selected in this invention can effectively adjust the foam structure of the pharmaceutical agent and improve its dispersibility. More preferably, the Tween surfactant is Tween 80.
[0016] As a preferred embodiment, the flotation collector is prepared by reacting raw materials including soluble inorganic base, fatty acid, hydroxamic acid, polyoxyethylene polyoxypropylene ether block copolymer and Tween surfactant in solution.
[0017] As a preferred embodiment, the preparation method of the flotation collector includes the following steps: 1) Dissolve the soluble inorganic base in an appropriate amount of water to prepare solution A; 2) Slowly add fatty acids to solution A, and heat and stir to prepare solution B; 3) Add hydroxamic acid, polyoxyethylene polyoxypropylene ether block copolymer and Tween surfactant to solution B, and continue heating and stirring until the reaction is complete and a homogeneous solution is formed to obtain the flotation collector.
[0018] As a preferred embodiment, the heating and stirring temperature in steps 2) and 3) is 70~100℃, and the time is 20~50min. At the selected temperature, the components in the collector can fully react to a stable state.
[0019] The present invention also provides an application of a flotation collector for the flotation of low-grade spodumene.
[0020] As a preferred embodiment, the low-grade spodumene flotation process involves sequentially crushing, grinding, and slurry conditioning the raw spodumene ore, then activating it with an activator containing metal ions to obtain an activated slurry; the activated slurry is then subjected to aeration flotation with the low-grade spodumene flotation collector to obtain spodumene concentrate and spodumene tailings.
[0021] This invention combines flotation collectors with specific flotation processes, enabling the upgrading of low-grade spodumene flotation while maintaining high recovery rates with the use of small amounts of collectors.
[0022] As a preferred embodiment, the particle size of the crushed spodumene ore is -3mm.
[0023] As a preferred embodiment, sodium carbonate is added during the grinding process. The purpose of adding an appropriate amount of sodium carbonate in this invention is to adjust the pH of the slurry to enhance the scrubbing effect of the reagent on spodumene, increase the electrostatic repulsion between spodumene and impurity mineral particles, and improve the separation effect between mineral particles. The dosage of sodium carbonate in this invention ranges from 1 to 3 kg / t.
[0024] As a preferred embodiment, the conditions for pulp conditioning are: pH 8-11 and pulp concentration 30-50%. The reagents used to adjust the pH of the pulp in this invention are sodium carbonate and sodium hydroxide; more preferably, the pH is 9-10 and the pulp concentration is 35-45%. As a preferred embodiment, the activator containing metal ions is represented by calcium and magnesium ions, and its dosage varies from 0-1000 g / t depending on the hardness of the beneficiation water and the properties of the ore. During the flotation process of spodumene minerals, the added metal ion activator introduces metal cations onto the surface of spodumene. These cations can react with the negative charge on the surface of the spodumene mineral, changing the charge state of the mineral surface, making it easier for the flotation agent to adsorb onto the mineral surface. Simultaneously, these cations can also promote the oleophilicity of the mineral surface and reduce its hydrophilicity. This change in wettability facilitates the interaction between mineral particles and the flotation agent, making the mineral particles easier to capture by the flotation agent and discharged with the froth during the flotation process. Further preferred activators are calcium chloride and / or magnesium chloride, with a dosage of 100~500g / t.
[0025] As a preferred embodiment, the aerated flotation includes one roughing stage, at least one cleaning stage, and at least one sweeping stage.
[0026] As a preferred embodiment, the collector dosage in the roughing process is 600-1000 g / t; no collector is added in the cleaning process; and the collector dosage in the scavenging process is 150-600 g / t. More preferably, the collector dosage in the roughing process is 600-800 g / t, and the collector dosage in the scavenging process is 300-500 g / t. The collector dosage in the flotation process of this invention is relatively low, which can significantly reduce production costs while ensuring the grade and recovery rate of spodumene.
[0027] Compared with the prior art, the present invention has the following beneficial effects: 1) The flotation collector provided by this invention has strong collecting ability and good selectivity. It improves the reactivity of fatty acids by saponifying fatty acid components with soluble inorganic bases. Combined with the chelating effect of hydroxamic acid, the foam adjustment effect of polyoxyethylene polyoxypropylene ether block copolymer, and the emulsifying effect of Tween surfactants, it significantly improves the grade and recovery rate of low-grade spodumene flotation concentrate, as well as production stability, without desliming treatment.
[0028] 2) By combining the flotation collector and flotation process of this invention, when the Li₂O grade of the raw ore is 0.6-1.0%, the grade of spodumene concentrate can reach 4.8-5.8%, with a recovery rate of 70-85%; when the Li₂O grade of the raw ore is 1.0-1.8%, the Li₂O grade of spodumene concentrate can reach 5.8-6.6%, with a recovery rate of 85-95%. This reagent and process not only greatly reduces the amount of reagent used in spodumene ore but also improves flotation efficiency. Attached Figure Description
[0029] Figure 1 This is a process flow diagram of the flotation process of the present invention. Detailed Implementation
[0030] To better understand the present invention, the following embodiments further illustrate the invention, but the scope of the invention is not limited to these embodiments. Other substitutions, modifications, variations, and deletions can be made to the design, operating conditions, and parameters of the following exemplary embodiments without departing from the spirit of the invention. All such modifications should be included within the scope of the invention. The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values; these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0031] The present invention will now be described with reference to specific embodiments.
[0032] Example 1 Add 17g of sodium carbonate to 90g of water and stir thoroughly until completely dissolved. Add 50g of oleic acid to the resulting sodium carbonate solution and heat and stir at 90℃ to ensure complete reaction. Then add 10g of C7~C9 alkyl hydroxamic acid, 3g of Pluronic L61, and 10g of Tween 80, and continue heating and stirring to obtain a homogeneous solution, which is the low-grade spodumene flotation collector. When using, dilute it to a specific concentration.
[0033] Example 2 Add 7g of sodium hydroxide to 90g of water and stir thoroughly until completely dissolved. Add 65g of soybean oleic acid to the resulting sodium hydroxide solution and heat and stir at 90℃ to ensure complete reaction. Then add 9g of benzohydroxyxamic acid, 3g of Pluronic L64, and 6g of Tween 80 in sequence, and continue heating and stirring to mix evenly. The resulting homogeneous solution is the low-grade spodumene flotation collector, which can be diluted to a specific concentration for use.
[0034] Application Example 1 The spodumene ore was ground to a thickness of -0.074mm with a content of 62%. Sodium carbonate was added to adjust the pulp pH to 9.5. Figure 1 The flotation process shown was tested. The collector was the one obtained in Example 1. The amount of calcium chloride activator in the roughing stage was 250 g / t, and the amount of collector was 700 g / t. The amount of calcium chloride in scavenging stage I was 100 g / t, and the amount of collector was 300 g / t. The amount of collector in scavenging stage II was 150 g / t. The flotation parameters are shown in Table 1.
[0035] Table 1. Flotation Indicators of Novel Collector in Yelonggou Lithium Spodumene Mine
[0036] Application Comparative Example 1 The raw materials and processes were the same as in Application Example 1, except that other combined reagents were used to replace the novel low-grade spodumene flotation collector. Sodium carbonate was added in the same amount as in Example 1 for saponification. The experimental results are shown in Table 2.
[0037] Table 2 Flotation Indicators of Yelonggou Spodumene Mine
[0038] Note: Hydroxyxamic acids in Table 2 are C7~C9 alkyl hydroxyxamic acids.
[0039] Comparing the results in Tables 1 and 2, it is clear that no component of the collector is indispensable. Within a certain dosage range, hydroxamic acid has a positive effect on improving the recovery and grade of spodumene. Pluronic L61 and Tween 80 have a significant impact on the flotation froth state of the collector, which can significantly affect flotation indicators. When Pluronic L61 is added, the flotation froth becomes more brittle, resulting in a higher grade of flotation concentrate, but a lower yield and recovery. Tween 80 has a positive effect on stabilizing the froth and improving the dispersibility and stability of the collector.
[0040] Application Example 2 The experimental procedure is as follows Figure 1 As shown, the spodumene ore was ground to a fineness of -0.074 mm with a content of 70%, the pulp pH was adjusted to 9.8, and the collector was the one obtained in Example 2. The roughing fraction used 400 g / t of calcium chloride and 800 g / t of collector; the scavenging fraction I used 200 g / t of calcium chloride and 300 g / t of collector; and the scavenging fraction II used 150 g / t of collector. The flotation parameters are shown in Table 3.
[0041] Table 3 Flotation Indicators of Novel Collectors for Spodumene Mines in Xinjiang
[0042] Application Comparative Example 2 The raw materials and processes were the same as in Application Example 2, except that other combined reagents were used to replace the novel low-grade spodumene flotation collector. Sodium hydroxide was added in the same amount as in Example 2 for saponification. The experimental results are shown in Table 4.
[0043] Table 4 Flotation Indicators for Spodumene Ore in Xinjiang
[0044] Note: Hydroxyxamic acid in Table 4 refers to benzohydroxyxamic acid.
[0045] Comparing the results in Tables 3 and 4, it can be seen that the absence of any component in the collector will reduce the recovery rate, grade and yield of spodumene flotation to varying degrees.
Claims
1. A flotation collector, characterized in that: It is obtained by reacting the following raw materials in parts by weight: 7-30 parts of soluble inorganic base, 50-70 parts of fatty acid, 5-15 parts of hydroxamic acid, 2-10 parts of polyoxyethylene polyoxypropylene ether block copolymer, 5-20 parts of Tween surfactant, and 60-100 parts of water. The hydroxamic acid is at least one of alkyl hydroxamic acid, salicylic acid, benzyl hydroxamic acid, naphthyl hydroxamic acid, and amide hydroxamic acid, which has a carbon chain length greater than 4. The preparation method of the flotation collector includes the following steps: 1) Dissolve the soluble inorganic base in an appropriate amount of water to prepare solution A; 2) Slowly add fatty acids to solution A, and heat and stir to prepare solution B; 3) Add hydroxamic acid, polyoxyethylene polyoxypropylene ether block copolymer and Tween surfactant to solution B, and continue heating and stirring until the reaction is complete and a homogeneous solution is formed to obtain the flotation collector. The heating and stirring temperature in steps 2 and 3 is 70~100℃, and the time is 20~50min.
2. The flotation collector according to claim 1, characterized in that: The fatty acid includes at least one of long-chain fatty acids with a carbon chain length greater than 12.
3. The flotation collector according to claim 1, characterized in that: The polyoxyethylene polyoxypropylene ether block copolymer is at least one of the Pluronic series L31, L35, L42, L43, L44, L45, L61, L62, L63, L64, P65, P84, F38 and F68.
4. The flotation collector according to claim 3, characterized in that: The Tween surfactants include at least one of Tween 20, Tween 21, Tween 40, Tween 60, Tween 61, Tween 80, Tween 81 and Tween 85.
5. The application of the flotation collector according to any one of claims 1 to 4, characterized in that: It is used in the flotation of low-grade spodumene.
6. The application of the flotation collector according to claim 5, characterized in that: After the raw spodumene ore is crushed, ground and slurry prepared in sequence, an activator containing metal ions is added to activate it to obtain an activated slurry. The activated slurry is then added to the flotation collector for aeration flotation to obtain spodumene concentrate and spodumene tailings.
7. The application of the flotation collector according to claim 6, characterized in that: Sodium carbonate is added during the grinding process; The grinding fineness is -0.074mm, and the content is 55~75%; The conditions for the slurry conditioning treatment are: pH 8-11 and slurry concentration 30-50%.
8. The application of the flotation collector according to claim 7, characterized in that: The pneumatic flotation includes one roughing stage, at least one cleaning stage, and at least one scavenging stage; The amount of collector used in the roughing process is 600~1000g / t; No collectors are added during the selection process; The amount of collector used in the scavenging process is 150~600g / t.
Citation Information
Patent Citations
Low-temperature-resistant mixed collector for synchronous recovery of lithium, beryllium, tantalum and niobium
CN108927289A
Coarse-grain spodumene enhanced flotation collecting agent and application
CN115213019A
Low-grade lepidolite ore flotation collecting agent and preparation method and application thereof
CN116967017A
Mercaptide microemulsion collectors for mineral flotation
WO2024006130A1