Laser processing system and wafer laser thinning method
By employing a non-contact thinning method using a laser processing system, combined with mapping functions and staged laser parameter control, the problems of mechanical damage, low efficiency, and high cost in wafer thinning have been solved, achieving a damage-free, low-cost, and highly efficient wafer thinning effect.
Patent Information
- Application Number
- CN202410171913.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-07
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-02-07
AI Technical Summary
In existing technologies, wafer thinning processes suffer from mechanical damage, low efficiency, and high costs. In particular, grinding wheel methods lead to decreased device reliability and high consumable costs.
Non-contact thinning is achieved using a laser processing system. By establishing a mapping function relationship between laser energy density and ablation depth, the laser parameters are controlled in stages to thin the wafer. This includes real-time surface profile control in the first stage and low laser energy density scanning optimization in the second stage.
This technology enables wafer thinning without mechanical damage, reducing costs and improving thinning efficiency, surface uniformity, and roughness to meet the requirements of subsequent process steps.
Smart Images

Figure CN117961308B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of laser processing technology, specifically to a laser processing system and a method for laser thinning of wafers. Background Technology
[0002] Monocrystalline silicon is widely used in the semiconductor industry, primarily in the fabrication of wafers. During wafer fabrication, to achieve a standard thickness for subsequent processes, the wafer needs to be thinned on both sides. Currently, the main industrial method for wafer thinning is grinding with abrasive wheels. This technology uses high-hardness abrasive grains bonded to the grinding wheel to cut, etch, and scratch the wafer. Wafers thinned using this technique suffer mechanical damage, potentially leading to decreased device reliability. Furthermore, grinding is inefficient, and the grinding wheels and grinding fluids used are extremely expensive consumables, significantly increasing the cost of grinding-based thinning. Summary of the Invention
[0003] The purpose of this application is to provide a laser processing system and a wafer laser thinning method, which thins the wafer through a non-contact processing method, without causing mechanical damage to the wafer surface, with low thinning cost and improved thinning efficiency.
[0004] One aspect of this application provides a wafer laser thinning method, including performing an ablation test on the wafer to establish a mapping function relationship between the surface ablation depth of the wafer and the laser energy density, and determining the optimized parameters of the laser module;
[0005] Obtain the surface height profile data of the wafer scanned by the height profile scanning module;
[0006] Based on the mapping function relationship and the surface height profile data, the laser module is controlled to emit laser light toward the wafer with thinning parameters to perform the first stage of thinning processing;
[0007] The laser module is controlled to emit the laser onto the wafer using the optimized parameters and in conjunction with a preset scanning path to perform the second stage of roughness optimization processing.
[0008] The thinning parameters and the optimization parameters include the laser wavelength, the laser energy density, and the spot overlap rate.
[0009] Optionally, the ablation test on the wafer to establish a mapping function relationship between the surface ablation depth of the wafer and the laser energy density, and to determine the optimized parameters of the laser module, includes:
[0010] The laser module is controlled to emit lasers toward the surface of the wafer at different laser energy densities to perform ablation tests.
[0011] Data on the ablation depth of regions corresponding to different laser energy densities were collected.
[0012] The mapping function relationship is obtained by fitting the data of the laser energy density and the ablation depth.
[0013] Optionally, the ablation test on the wafer to establish a mapping function relationship between the surface ablation depth of the wafer and the laser energy density, and to determine the optimized parameters of the laser module, includes:
[0014] The surface of the ablated wafer is observed using an optical microscope. When the surface of the wafer is bright white and has a regular morphology, the current laser parameters are within the range of the optimized parameters.
[0015] Optionally, a polynomial scheme is used to fit the laser energy density and ablation depth data, and the mapping function relationship between the surface ablation depth of the wafer and the laser energy density satisfies: H = k1 × F 2 +k2×F-k3, where H is the surface ablation depth of the wafer, F is the laser energy density of the laser module, and k1, k2, and k3 are mapping constants.
[0016] Optionally, controlling the laser module to emit laser light towards the wafer with thinning parameters according to the mapping function relationship and the surface height profile data to perform the first stage of thinning processing includes:
[0017] The laser module is controlled to scan the wafer multiple times, so that the minimum point of the surface height profile of the wafer is thinned in a single operation by d1 = (1 / 10 ~ 1 / 3) × D0, where D0 is the preset total thinning amount of the wafer.
[0018] After each thinning process, the thinning amount and height uniformity are detected. If the requirements are not met, the surface height profile data is collected again. Based on the mapping function relationship and the surface height profile data, the laser module is controlled to emit the laser towards the wafer with the thinning parameters to perform the thinning process.
[0019] Optionally, the thinning parameters include a spot overlap rate ranging from 40% to 80% and a laser energy density ranging from 30 J / cm². 2 ~60J / cm 2 .
[0020] Optionally, controlling the laser module to emit the laser onto the wafer using the optimized parameters and in conjunction with a preset scanning path to perform a second stage of roughness optimization processing includes:
[0021] The laser module is controlled to emit laser light toward the wafer along mutually perpendicular scanning paths. The surface roughness of the wafer in the second stage is lower than Sa, where Sa is a preset roughness standard for the wafer.
[0022] Optionally, the optimization parameters include a spot overlap rate ranging from 60% to 90% and a laser energy density ranging from 8 J / cm². 2 ~18J / cm 2 .
[0023] Optionally, the laser is a green laser or an infrared laser, with a laser pulse width of ns and a spot size of 10μm to 300μm.
[0024] In another aspect of this application, a laser processing system is provided for wafer processing according to the above-described wafer laser thinning method. The system includes a laser processing module, a height profile scanning module, and a control module. The control module is electrically connected to both the laser processing module and the height profile scanning module. It also includes a moving platform on which the wafer is placed. The height profile scanning module scans the surface height profile of the wafer and feeds it back to the control module. The control module controls the laser processing module to emit a laser beam toward the wafer on the moving platform to reduce the thickness of the wafer and perform surface roughness optimization processing on the wafer.
[0025] The laser processing system provided in this application includes a height profile scanning module that scans the surface height profile of the wafer and feeds it back to the control module. The control module then controls the laser processing module to emit a laser beam toward the wafer on the moving platform to reduce the wafer's thickness and optimize its surface roughness. This application employs laser thinning, which offers advantages such as no mechanical damage to the wafer after thinning, low cost, and high efficiency. The surface uniformity and roughness of the thinned wafer are crucial technical standards that directly affect subsequent wafer fabrication processes. This application uses a non-contact laser processing method to thin the wafer, avoiding mechanical damage to the wafer surface, reducing thinning costs, and improving thinning efficiency.
[0026] The wafer laser thinning method adopts a staged thinning approach. In the first stage, the laser energy is adjusted in real time based on the surface contour to ensure the uniformity of the surface height and the amount of thinning after thinning. In the second stage, a low laser energy density and overlap rate combined with a unique scanning method can effectively optimize the surface roughness. Attached Figure Description
[0027] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the embodiments of this application will be briefly introduced below. It should be understood that the following drawings only show some embodiments of this application and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0028] Figure 1 This is a schematic diagram of the laser processing system structure provided in this embodiment;
[0029] Figure 2 This is a schematic diagram of the wafer laser thinning method provided in this embodiment;
[0030] Figure 3 This is a second-stage scanning path diagram of the wafer laser thinning method provided in this embodiment;
[0031] Figure 4 This is a graph showing the mapping function relationship between the surface ablation depth and the laser energy density in the wafer laser thinning method embodiment provided in this example;
[0032] Figure 5 This is a height difference diagram after the first stage of thinning in the wafer laser thinning method embodiment provided in this example;
[0033] Figure 6 This is a surface roughness diagram after the first stage of thinning in the wafer laser thinning method embodiment provided in this example;
[0034] Figure 7 This is a surface roughness diagram after the second stage of processing in the wafer laser thinning method embodiment provided in this example.
[0035] Icons: 1-Laser; 2-Galvanometer; 3-Field lens; 4-Height profile scanning module; 5-Wafer; 6-Moving platform; 7-Dust removal system. Detailed Implementation
[0036] The technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings.
[0037] In the description of this application, it should be noted that the terms "inner" and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, or the orientation or positional relationship commonly used when the product is in use. They are used only for the convenience of describing this application and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application. Furthermore, the terms "first," "second," etc., are used only to distinguish descriptions and should not be construed as indicating or implying relative importance.
[0038] It should also be noted that, unless otherwise explicitly specified and limited, the terms "setup" and "connection" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this application based on the specific circumstances.
[0039] Please refer to Figure 1 As shown, this application provides a laser processing system that thins a wafer 5 using a non-contact processing method. The thinning process does not cause mechanical damage to the surface of the wafer 5. At the same time, the laser thinning process does not require additional consumables, resulting in low thinning costs. Furthermore, by setting up multiple lasers 1 to perform thinning processing simultaneously, the thinning efficiency can be greatly improved.
[0040] Specifically, the laser processing system provided in this application includes: a laser processing module, a height profile scanning module 4, and a control module. The control module is electrically connected to the laser processing module and the height profile scanning module 4, respectively. It also includes a moving platform 6, on which a wafer 5 is disposed. The height profile scanning module 4 scans the surface height profile of the wafer 5 and feeds it back to the control module. The control module controls the laser processing module to emit laser light toward the wafer 5 on the moving platform 6 to reduce the thickness of the wafer 5 and perform roughness optimization processing on the wafer 5.
[0041] The moving platform 6 is used to support the wafer 5. The moving platform 6 has vacuum adsorption capability to fix the wafer 5 and ensure the uniformity of the initial height of the wafer 5. The moving platform 6 can translate in the x, y and z directions.
[0042] The laser processing module includes a laser 1, a galvanometer 2, and a field mirror 3 arranged in sequence. The laser emitted from the laser 1 is directed onto the wafer 5 through the galvanometer 2 and the field mirror 3.
[0043] Laser 1 is used to output a laser beam, which is then irradiated onto the surface of wafer 5 by galvanometer 2 and field mirror 3 after the optical path is deflected by two mirrors. This achieves the thickness reduction process of wafer 5 and the roughness optimization process of wafer 5.
[0044] The galvanometer 2 can control the movement of the laser in the x and y planes, and the laser scanning speed is adjusted by the galvanometer 2 in conjunction with the field mirror 3.
[0045] In a practical application, the wafer 5 is first placed on one side of the height profile scanning module 4, allowing the height profile scanning module 4 to scan and acquire the height profile data of the wafer 5 surface to obtain the initial data of the height profile of the wafer 5 surface. For example, the height profile scanning module 4 can be a spectral confocal sensor.
[0046] Then, the wafer 5 is moved to the corresponding position of the laser processing module via the moving platform 6, so that the laser emitted by the laser 1 passes through the galvanometer 2 and the field mirror 3 in sequence and is emitted towards the wafer 5. Based on the initial data of the height profile of the wafer 5 surface obtained by the height profile scanning module 4, and the final thickness to be reduced of the wafer 5, the parameters of the laser emitted by the laser 1, such as the laser energy density and irradiation time, can be controlled so that the wafer 5 is thinned by laser irradiation, and finally a product of the required thickness is obtained. In addition, the wafer 5 is also subjected to roughness optimization processing so that the surface of the wafer 5 after processing meets the roughness requirements.
[0047] During this process, automatic control is performed by the control module. The control module controls the height profile scanning module 4 to scan the surface height profile of the wafer 5 and receives the scanned surface height profile of the wafer 5. Then, the control module controls the moving platform 6 to move the wafer 5 to the corresponding position of the laser module and controls the laser to emit laser light towards the wafer 5 with the required parameters.
[0048] It should be noted that the laser processing module and the height contour scanning module 4 can also be set at the same workstation, for example, above the moving platform 6, to perform the aforementioned surface height contour scanning and laser processing sequentially.
[0049] Furthermore, the control module mainly includes a height profile data processing unit, a galvanometer 2 control unit, a laser 1 control unit, and a computer. After receiving the surface profile data of wafer 5, the height profile data processing unit, combined with the established mapping function relationship between laser ablation depth and laser energy density, generates laser energy density data during the scanning process. The galvanometer 2 control unit, through the deflection of the galvanometer 2 lenses and in conjunction with the field mirror 3, can adjust the laser scanning speed and spacing during the thinning process. The laser control group adjusts the laser energy in real time based on the surface height profile of wafer 5 during the thinning process.
[0050] During the laser thinning process of the wafer 5, a dust removal system 7 is also installed on the moving platform 6. The dust removal system 7 is located on one side of the wafer 5 and removes dust from the wafer 5 during processing.
[0051] Since a large amount of material is removed from wafer 5 during thinning, the generated dust will directly affect the absorption of laser energy by wafer 5. If the dust falls into the unprocessed area, it will cause problems such as uneven height and high roughness after processing. Therefore, this application sets up a dust removal system 7 consisting of two parts, air blowing and dust extraction, which are placed on both sides of wafer 5 to extract the dust generated during the thinning process.
[0052] Therefore, in the laser processing system provided in this application embodiment, the height profile scanning module 4 scans the surface height profile of the wafer 5 and feeds it back to the control module. The control module controls the laser processing module to emit a laser towards the wafer 5 on the moving platform 6 to reduce the thickness of the wafer 5 and perform roughness optimization processing on the wafer 5. This application uses laser thinning processing, which has the advantages of no mechanical damage to the wafer 5 after thinning, low thinning cost, and high efficiency. The surface height uniformity and roughness of the wafer 5 after thinning are very important technical standards, which will directly affect the subsequent process of wafer 5. This application uses laser processing, a non-contact processing method, to thin the wafer 5, which will not cause mechanical damage to the surface of the wafer 5, has low thinning cost, and can also improve thinning efficiency.
[0053] Based on this, the embodiments of this application also provide a wafer laser thinning method, which adopts a staged processing approach. In the first stage, the laser energy is adjusted in real time based on the surface contour to ensure the uniformity of the surface height and the amount of thinning after thinning. In the second stage, a low laser energy density and overlap rate are combined with a unique scanning method to effectively optimize the surface roughness.
[0054] Specifically, please refer to Figure 2 As shown in the embodiments of this application, the wafer laser thinning method uses a silicon wafer as an example for wafer 5. Specifically, the method includes:
[0055] S100: Perform an ablation test on wafer 5 to establish a mapping function relationship between the surface ablation depth of wafer 5 and the laser energy density, and determine the optimized parameters of the laser module.
[0056] First, the laser module is controlled to emit lasers at different energy densities toward multiple areas on the surface of wafer 5 to perform ablation tests.
[0057] This application is not limited to this; lasers can also be emitted separately from the surfaces of multiple wafers 5 to perform ablation tests.
[0058] Secondly, data on the ablation depth of regions corresponding to different laser energy densities were collected;
[0059] For example, in this application, a laser 1 can be used to perform an ablation test on a wafer 5. During the test, the laser spot overlap rate is kept consistent, and the laser energy density is varied to scan multiple areas of the wafer 5. The ablation depth H of the corresponding area under different laser energy densities Ed is measured using a laser confocal microscope. The measurement can be taken three times and the average value is taken. By changing the laser spot overlap rate and performing the ablation test as described above, the ablation depth of the corresponding area under different laser energy densities Ed with different laser spot overlap rates can be obtained.
[0060] Finally, the data on laser energy density and ablation depth are fitted to obtain the mapping function relationship.
[0061] After obtaining the corresponding data of laser energy density Ed and ablation depth H, the ablation pit depth H and laser energy density Ed are fitted to obtain the corresponding mapping function relationship. This mapping function relationship is then input into the control module for subsequent processing. Specifically, a polynomial approach is used to fit the laser energy density and ablation depth data, establishing a mapping function relationship between the surface ablation depth of wafer 5 and the laser parameters that satisfies: H = k1 × F 2 +k2×F-k3, H is the surface ablation depth of wafer 5, F is the laser energy density of the laser module, k1, k2, and k3 are mapping constants, and k1, k2, and k3 can be set according to different situations.
[0062] During the ablation test of wafer 5, in addition to establishing the mapping function relationship between the surface ablation depth of wafer 5 and the laser parameters, this step can also determine the optimization parameters of the laser module in the second stage through the ablation test, so as to be used in the subsequent steps for the second stage roughness optimization processing.
[0063] In practice, the surface of wafer 5 after ablation is observed. When the surface of wafer 5 is bright white and has a regular arrangement, the current laser parameters are used as the selection range of the laser module's optimization parameters during the second stage of roughness optimization processing.
[0064] As will be understood by those skilled in the art, the wafer 5 used in step S100 for the ablation test is called the test wafer 5, and the wafer 5 used in subsequent steps S110 to S130 is called the wafer to be processed 5. The test wafer 5 and the wafer to be processed 5 can be the same wafer 5 or different individuals from the same type of wafer 5. Furthermore, during the ablation test, an area can be divided on a single wafer 5 for ablation testing, or ablation testing can be performed on multiple wafers 5. Those skilled in the art will know that by selecting different laser parameters for the ablation test, such as wavelength, spot overlap rate, pulse width, and spot size, a corresponding mapping function relationship can be obtained, allowing for the selection of thinning parameters and optimization parameters.
[0065] S110: Obtain the surface height profile data of the wafer 5 scanned by the height profile scanning module 4.
[0066] The initial data of the height profile of wafer 5 surface were obtained by scanning and acquiring the height profile data of wafer 5 surface using a spectral confocal sensor.
[0067] S120: Based on the mapping function relationship and surface height profile data, control the laser module to emit laser towards wafer 5 with thinning parameters to perform the first stage of rough thinning processing.
[0068] Entering the first stage of formal processing, the laser processing parameters can be obtained based on the initial data of the mapping function relationship and surface height contour data. These laser parameters include, but are not limited to: when the spot size is in the range of 10μm to 300μm, thinning parameters include a spot overlap rate ranging from 40% to 80%, and a laser energy density ranging from 30J / cm². 2 ~60J / cm 2 .
[0069] The entire thinning process is set with a thinning amount of D0, which is the preset total thinning amount for wafer 5. The surface roughness after thinning is set not to exceed Sa. The first stage of thinning begins based on the surface height profile data of wafer 5. To achieve the set thinning amount in the first stage, multiple scans are required. The instantaneous high temperature generated by the laser vaporizes wafer 5, achieving thinning. The laser module is controlled to scan wafer 5 multiple times, ensuring that the single thinning amount d1 at the lowest point of the surface height profile of wafer 5 satisfies d1 = (1 / 10 ~ 1 / 3) × D0.
[0070] Understandably, during thinning, the single thinning amount is smallest at the lowest point of the wafer 5 surface contour and largest at the highest point. The single thinning amount of the entire contour can be obtained from the aforementioned initial height data and the single thinning amount at the lowest point. During processing, the laser energy is lowest when it scans to the lowest point of the wafer 5 surface contour, and the corresponding laser energy density is the laser energy density at the ablation depth d1 in the ablation test. By controlling the laser energy density at other height positions of wafer 5 according to the mapping relationship between ablation depth and laser energy density, the surface contour height uniformity after thinning can be effectively improved.
[0071] After each thinning process, the thinning amount and height uniformity are checked. If the requirements are not met, the surface height profile data is collected again and processed. When the surface height uniformity meets the requirements and the thinning amount reaches D0, the first stage of processing ends.
[0072] Specifically, the surface height uniformity index can be measured by the height difference between the highest and lowest points. When the test reaches or falls below the set height difference, the surface height uniformity is considered to meet the requirements.
[0073] S130: Controls the laser module to optimize parameters and, in conjunction with a preset scanning path, performs the second stage of surface roughness optimization processing by emitting laser from wafer 5.
[0074] The second stage employs low laser energy density and a specific spot overlap rate, combined with a scanning method where each two adjacent scans are perpendicular to each other. Figure 3Laser scanning is performed using mutually perpendicular horizontal S-shaped scanning paths and vertical S-shaped scanning paths. During this stage, the surface temperature of wafer 5 is controlled to be between the melting point and the vaporization point during the laser processing. The scanning process causes the rough surface of wafer 5 to melt and then solidify, thereby optimizing the surface roughness.
[0075] As a preferred embodiment, in step S100, after controlling the laser module to emit lasers at different laser energy densities towards multiple areas on the surface of wafer 5 for ablation testing, the method further includes observing the surface of wafer 5 using a microscope. When the surface of wafer 5 is bright white and exhibits a regularly arranged morphology, it indicates that the surface temperature during laser processing of wafer 5 is between the melting temperature and the vaporization point. The laser parameters at this point are then set to the laser parameter selection range for the second stage of roughness optimization, i.e., the optimized parameters. These optimized parameters include, but are not limited to: when the spot size is within the range of 10 μm to 300 μm, the optimized parameters include a spot overlap rate range of 60% to 90% and a laser energy density range of 8 J / cm². 2 ~18J / cm 2 During this scanning phase, the laser energy remains constant. After each scan, the surface roughness is measured. When the roughness is equal to or lower than the set roughness Sa, the entire thinning process ends.
[0076] It should be noted that the aforementioned spot size refers to the diameter when the spot is a Gaussian spot, and its width when the spot is a shaped square spot. When the spot is of other shaped forms, the spot size is the conventional size characterized in this field.
[0077] Preferably, the laser is an ultraviolet or infrared laser with a nanosecond or femtosecond pulse width. During the above thinning process, the wafer 5 is held in place by the moving platform 6, ensuring high uniformity before the thinning process; the dust removal system 7 on both sides of the wafer 5 on the moving platform 6 extracts the dust generated during the thinning process.
[0078] The method is described below with reference to specific embodiments, which are as follows:
[0079] First, a surface ablation test was conducted. The laser used had a wavelength of 1064nm, a pulse width of 100ns, and a focused circular Gaussian spot diameter of 57μm. The initial thickness of wafer 5 was about 900μm, and the required thinning amount was 30μm. The surface roughness after thinning should not exceed 1.5μm.
[0080] In the ablation test, a scanning area of 5mm × 5mm was set, a large spot overlap rate of 70% was selected, and a repetition frequency of 33kHz was set. The scanning speed v = 564.3mm / s and the scanning line spacing L = 0.0171mm were determined. Sixteen sets of laser energies were used to scan wafer 5, and the ablation depth of the 16 ablation areas was measured using a laser confocal microscope. The ablation depth data and the corresponding laser energy density were then fitted to obtain the functional relationship between the ablation depth H and the laser energy density Ed, as follows:
[0081] H = -0.0122 × F 2 +1.42482×F-17.613;
[0082] Function curves as follows Figure 4 The ablation depth and laser energy density function obtained above are input into the control module.
[0083] The surface height profile data of wafer 5 was acquired using a spectral confocal sensor, and then the first stage of thinning was initiated. The laser spot overlap rate in this stage was maintained at 70%, consistent with the ablation test. The first-stage thinning amount was set to 30 μm, performed in 5 passes, with a single scan thinning amount of 6 μm. Therefore, the height of the lowest point on the surface profile of wafer 5 decreased by 5 μm after the first thinning process. The laser energy density at this point corresponds to the ablation depth of 5 μm in the function relationship. During the thinning process at other locations on wafer 5, the laser energy density changed in real time with the surface profile height of wafer 5 according to the mapping relationship between ablation depth and laser energy density. The laser energy density and the surface profile height of wafer 5 were positively correlated. After the scan was completed, the surface height uniformity was checked, and the surface height uniformity was improved.
[0084] After the first thinning process, the surface height profile was scanned and acquired. A second thinning process was then performed based on this profile. After the second processing, the surface uniformity met the requirements. Subsequent processing ensured sufficient thinning, and after three more thinning processes, the thinning amount reached approximately 30 μm. At this point, the surface roughness was 3.2 μm. Figure 5 , Figure 6 The first phase of thinning has ended.
[0085] The second stage requires reducing the roughness to 1.5 μm. This stage uses a spot overlap rate of 60% and a laser energy density of 12 J / cm². 2 The scanning directions were perpendicular to each other in every two adjacent scans. The surface roughness was checked after each processing. After three processing cycles, the surface roughness decreased to 1.3 μm, which met the requirements. Figure 7 The entire thinning process is now complete.
[0086] In summary, the laser processing system and wafer laser thinning method provided in this application, due to the non-contact processing characteristics of lasers, do not cause mechanical damage to the wafer 5 during thinning. Furthermore, laser thinning does not require additional consumables, resulting in low operating costs. By using multiple lasers 1 simultaneously, the thinning efficiency can be significantly improved. The phased thinning approach involves: in the first phase, laser energy is adjusted in real-time based on the surface contour to ensure uniform surface height and thinning amount after thinning; in the second phase, low laser energy density and overlap rate combined with a unique scanning method effectively optimize surface roughness.
[0087] This wafer laser thinning method includes the same structure and beneficial effects as the laser processing system in the foregoing embodiments. The structure and beneficial effects of the laser processing system have been described in detail in the foregoing embodiments and will not be repeated here.
[0088] The above description is merely an embodiment of this application and is not intended to limit the scope of protection of this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the scope of protection of this application.
Claims
1. A wafer laser thinning method, characterized in that, The method includes: The wafer was subjected to ablation testing to establish the mapping function relationship between the surface ablation depth of the wafer and the laser energy density, and to determine the optimized parameters of the laser module. Obtain the surface height profile data of the wafer scanned by the height profile scanning module; Based on the mapping function relationship and the surface height profile data, the laser module is controlled to emit laser light toward the wafer with thinning parameters to perform the first stage of thinning processing; The laser module is controlled to emit the laser onto the wafer using the optimized parameters and in conjunction with a preset scanning path to perform the second stage of roughness optimization processing. The thinning parameters and the optimization parameters include the laser wavelength, the laser energy density, and the spot overlap rate; The laser is either green light or infrared laser; During the first stage of thinning, the laser spot overlap rate ranges from 40% to 80%, and the laser energy density ranges from 30 J / cm². 2 ~60J / cm 2 The wafer is thinned by vaporizing it using the instantaneous high temperature generated by the laser. The laser has the lowest energy when it scans to the lowest point of the wafer surface contour. The corresponding laser energy density is the laser energy density when the ablation depth is d1 in the ablation test. The laser energy density at other height positions of the wafer is controlled to change in real time with the height of the wafer surface contour according to the mapping relationship between the ablation depth and the laser energy density. During the second stage of roughness optimization processing, the spot overlap rate ranges from 60% to 90%, and the laser energy density ranges from 8 J / cm². 2 ~18J / cm 2 The temperature of the wafer surface is controlled to be between the melting point and the vaporization point during the laser processing. The scanning process causes the rough surface of the wafer to melt and then solidify.
2. The wafer laser thinning method according to claim 1, characterized in that, The ablation test on the wafer is performed to establish a mapping function relationship between the surface ablation depth of the wafer and the laser energy density, and to determine the optimized parameters of the laser module, including: The laser module is controlled to emit lasers toward the surface of the wafer at different laser energy densities to perform ablation tests. Data on the ablation depth of regions corresponding to different laser energy densities were collected. The mapping function relationship is obtained by fitting the data of the laser energy density and the ablation depth.
3. The wafer laser thinning method according to claim 2, characterized in that, The ablation test on the wafer is performed to establish a mapping function relationship between the surface ablation depth of the wafer and the laser energy density, and to determine the optimized parameters of the laser module, including: The surface of the ablated wafer is observed using an optical microscope. When the surface of the wafer is bright white and has a regular morphology, the current laser parameters are within the range of the optimized parameters.
4. The wafer laser thinning method according to any one of claims 1 to 3, characterized in that, A polynomial approach was used to fit the laser energy density and ablation depth data. The mapping function relationship between the surface ablation depth of the wafer and the laser energy density satisfies: H = k1 × F 2 +k2×F-k3, where H is the surface ablation depth of the wafer, F is the laser energy density of the laser module, and k1, k2, and k3 are mapping constants.
5. The wafer laser thinning method according to any one of claims 1 to 3, characterized in that, The step of controlling the laser module to emit laser light toward the wafer with thinning parameters according to the mapping function relationship and the surface height contour data to perform the first stage of thinning processing includes: The laser module is controlled to scan the wafer multiple times, so that the minimum point of the surface height profile of the wafer is thinned in a single operation by d1 = (1 / 10 ~ 1 / 3) × D0, where D0 is the preset total thinning amount of the wafer. After each thinning process, the thinning amount and height uniformity are detected. If the requirements are not met, the surface height profile data is collected again. Based on the mapping function relationship and the surface height profile data, the laser module is controlled to emit the laser towards the wafer with the thinning parameters to perform the thinning process.
6. The wafer laser thinning method according to any one of claims 1 to 3, characterized in that, The process of controlling the laser module to emit laser light from the wafer using the optimized parameters and in accordance with a preset scanning path to perform a second stage of roughness optimization includes: The laser module is controlled to emit laser light toward the wafer along mutually perpendicular scanning paths. The surface roughness of the wafer in the second stage is lower than Sa, where Sa is a preset roughness standard for the wafer.
7. The wafer laser thinning method according to claim 1, characterized in that, The laser pulse width is ns, and the spot size is 10μm to 300μm.
8. A laser processing system for processing wafers according to the wafer laser thinning method according to any one of claims 1 to 7, characterized in that, include: The system includes a laser processing module, a height profile scanning module, and a control module, with the control module electrically connected to both the laser processing module and the height profile scanning module. It also includes a moving platform on which a wafer is mounted. The height profile scanning module scans the surface height profile of the wafer and feeds it back to the control module. The control module controls the laser processing module to emit a laser beam toward the wafer on the moving platform to reduce the wafer's thickness and perform surface roughness optimization processing.
Citation Information
Patent Citations
Method and equipment for removing dielectric layer on surface of wafer by laser
CN115178882A
Green ultrafast laser beam wafer thinning method and system approximately perpendicular to wafer surface
CN116551189A
Laser polishing diamond surface microscopic landform and roughness simulation prediction analysis method
CN116631547A