A method for ultrasonic-assisted laser preparation of ultrafine piezoelectric nanoparticles
Ultrafine piezoelectric nanoparticles were prepared by ultrasound-assisted laser ablation and inert gas purging, which solved the problems of delivery efficiency and endocytosis caused by the large particle size in the existing technology. This method achieved the preparation of nanoparticles with high crystallinity and good biocompatibility, which are suitable for biomedical applications.
Patent Information
- Application Number
- CN202410185425.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-19
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-02-19
AI Technical Summary
Existing technologies make it difficult to prepare ultrafine piezoelectric nanoparticles with a particle size of less than 20 nm, which affects their delivery efficiency as drug carriers and their endocytosis effect, resulting in the nanoparticles mainly acting extracellularly.
Ultrafine piezoelectric nanoparticles were prepared by using ultrasound-assisted laser ablation combined with inert gas purging and filter membrane collection. The nanoparticles were formed by laser ablation and the particle size was refined and homogenized by ultrasound, combined with inert gas purging and solvent cleaning.
Highly crystalline ultrafine piezoelectric nanoparticles with a particle size of 5-20 nm were prepared. The process is simple, low-cost, suitable for the biomedical field, and suitable for mass production.
Smart Images

Figure CN117961310B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of nanomaterials technology, and specifically relates to a method for preparing ultrafine piezoelectric nanoparticles using ultrasound-assisted laser. Background Technology
[0002] The statements herein provide only background information in relation to this invention and do not necessarily constitute prior art.
[0003] Since the late 20th century, nanomaterials have received widespread attention and rapid development due to their unique physicochemical properties. In the biomedical field, nanomaterials, with their special surface properties, size effects, and structural characteristics, also show great promise in drug delivery, diagnostic imaging, tissue engineering, and biosensing. In drug delivery, nanoparticles, with their large specific surface area and surface activity, can be used as drug carriers to achieve targeted drug delivery within the body. Furthermore, the unique properties of nanoparticles can be utilized to regulate cells and tissues; for example, nanoparticles can disrupt bacterial cell membranes through endocytosis to achieve antibacterial effects, or their piezoelectric and photothermal properties can be used to target and regulate cell differentiation and functional expression. In diagnostic imaging, the unique magnetic resonance imaging, fluorescence imaging, or X-ray imaging properties of nanoparticles can be used to label biomolecules or cells, thereby achieving high-sensitivity and high-resolution imaging of biological tissues.
[0004] Bioelectricity within the body is a crucial component of the regenerative microenvironment and a key pathway for tissue response to external stimuli and the regulation of cell fate. For example, cell membrane potential plays a guiding role in stem cell differentiation, while electric fields mediate processes such as intercellular communication and tissue repair. The piezoelectric effect refers to the generation of microcurrents in materials under stimuli such as exogenous mechanical vibration and polarization. As a major component of human bone tissue, collagen fibers possess piezoelectric response characteristics, enabling the formation of an electrophysiological microenvironment within bone and facilitating the interconversion between mechanical stimulation and electrical energy, thereby maintaining normal metabolism and physiological activities in bone tissue. Therefore, the piezoelectric effect plays a vital role in bone formation, shaping, reconstruction, and functional expression. Studies have found that simulating the microcurrent environment within bone can enhance bone repair.
[0005] The fabrication of piezoelectric nanoparticles combines the effects of nanosize and piezoelectricity, holding significant potential for applications in the biomedical field. Particularly, it enables stem cell endocytosis of nanoparticles based on nanosize, allowing for effective regulation of stem cell differentiation through the piezoelectric effect. Existing research has identified several piezoelectric materials with piezoelectric effects, such as lithium tantalate (LiTaO3), lithium niobate (LiNbO3), and barium titanate (BaTiO3). The piezoelectric properties of these nanoparticles can be used to directly act on stem cells, promoting osteogenic processes through stimulation of voltage-gated calcium channels, activation of cell signal transduction pathways, and increased local blood flow. Furthermore, as nonlinear optical nanomaterials with frequency doubling effects, lithium niobate and lithium tantalate nanoparticles exhibit upconversion luminescence properties. Upconversion fluorescent nanomaterials possess unique advantages such as good photostability, minimal damage to organisms, low background fluorescence interference, and strong tissue penetration, making them excellent probe materials for in vivo fluorescence imaging, allowing for direct observation of gene expression and cellular activity in animals. Therefore, the upconversion luminescence properties of nanoparticles can also be used for in vivo imaging observation, such as real-time observation of the growth of bone tissue around the implant, which is beneficial for evaluating the bone integration effect around the implant.
[0006] Currently, the main methods for preparing piezoelectric nanoparticles include the sol-gel method, hydrothermal method, and solvothermal method. A literature search of existing technologies revealed that Chinese patents CN103787415A and CN103833079A disclose methods for preparing lithium tantalate nanoparticles using solvothermal and hydrothermal methods, respectively, with the diameter of the obtained lithium tantalate particles exceeding 100 nm. Chinese patent CN101602596A discloses a method for preparing lithium tantalate nanoparticles using the sol-gel method, with the diameter of the obtained lithium tantalate particles being approximately 30 nm. Chinese patent CN113209290A prepared barium titanate particles with a particle size of 100-150 nm using a hydrothermal method.
[0007] Therefore, existing methods for preparing piezoelectric nanoparticles result in larger particle sizes. This larger particle size affects their drug delivery efficiency and also impacts the endocytosis effect of cells and bacteria, causing the nanoparticles to primarily act extracellularly. However, for ultrafine piezoelectric nanoparticles with a diameter of less than 20 nm, cells or bacteria can significantly phagocytose them. Through endocytosis, the nanoparticles can directly act on intracellular organelles, thereby affecting cell function, such as inducing osteogenic or neurogenic differentiation of stem cells, or inducing bacterial apoptosis. However, current synthesis techniques are still insufficient for ultrafine piezoelectric nanoparticles with a diameter of less than 20 nm. Summary of the Invention
[0008] To address the shortcomings of existing technologies, the present invention aims to provide a method for preparing ultrafine piezoelectric nanoparticles using ultrasound-assisted laser technology, thus solving the problems mentioned in the background section. The preparation method provided by this invention is simple to operate, environmentally friendly, and produces ultrafine piezoelectric nanoparticles with uniform particle size and good biocompatibility, making it suitable for applications in biomedicine and other fields.
[0009] To achieve the above objectives, the present invention is implemented through the following technical solution:
[0010] In a first aspect, the present invention provides a method for preparing ultrafine piezoelectric nanoparticles by ultrasound-assisted laser, comprising the following steps: placing a ceramic boat containing piezoelectric material raw materials into a quartz tube having an outlet hole and an air inlet hole;
[0011] An ultrasonic transducer is fixed to the lower surface of a ceramic boat, and ultrasonic waves are applied to the ceramic boat.
[0012] Simultaneously, the piezoelectric material raw material is subjected to laser ablation. During the laser ablation process, inert gas is used for purging, and nanoparticles are collected using a filter membrane.
[0013] After laser ablation, the filter membrane is placed in a solvent for ultrasonic cleaning. The resulting nanoparticle suspension is then centrifuged, dried, and ultrafine piezoelectric nanoparticles are obtained.
[0014] Laser ablation utilizes laser irradiation to transfer heat to the surface of a material, causing instantaneous melting and vaporization. The recoil pressure generated by the vapor allows the molten material to be ejected and sputtered, forming nanoparticles. Ultrasound can produce a discharge effect, Marangoni effect, and acoustic cavitation effect on the solution within the laser ablation molten pool, promoting the sputtering of the laser ablation molten material and simultaneously promoting particle refinement and size uniformity.
[0015] In some embodiments, the piezoelectric material raw material is in the form of a block or powder.
[0016] Preferably, the piezoelectric material is lithium tantalate, lithium niobate, barium titanate, potassium sodium niobate, zinc oxide, titanium oxide, or aluminum zirconate titanate.
[0017] In some embodiments, during laser ablation, the wavelength of the laser is 355-1064 nm and the pulse width is 0.4-20 ns.
[0018] Preferably, the laser power density is 0.5-15.0 J / cm². 2 .
[0019] In some embodiments, the ultrasonic frequency is 20-50 kHz; the ultrasonic power is 10-1000 W.
[0020] In some embodiments, the inert gas is nitrogen or argon.
[0021] In some embodiments, the ultrafine piezoelectric nanoparticles are vacuum dried at a temperature of 20-50°C for 6-12 hours.
[0022] In some embodiments, the solvent is anhydrous ethanol or deionized water.
[0023] Secondly, the present invention provides an ultrafine piezoelectric nanoparticle prepared by the aforementioned preparation method.
[0024] In some embodiments, the ultrafine piezoelectric nanoparticles have a particle size of 5-20 nm and exhibit high crystallinity and sphericity.
[0025] The beneficial effects achieved by one or more embodiments of the present invention described above are as follows:
[0026] This invention employs ultrasonic-assisted high-energy pulsed laser ablation of piezoelectric material raw materials, followed by high-temperature in-situ gas-phase reaction to form highly crystalline ultrafine piezoelectric nanoparticles with a particle size of 5-20 nm, overcoming the technical challenges in preparing ultrafine piezoelectric nanoparticles. The process described in this invention is simple to operate, low in cost, and fast in preparation speed, making it suitable for mass production. Attached Figure Description
[0027] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.
[0028] Figure 1 This is a transmission electron microscope image of the lithium niobate ultrafine piezoelectric nanoparticles prepared in Example 1 of the present invention;
[0029] Figure 2 This is a transmission electron microscope image of the lithium tantalate ultrafine piezoelectric nanoparticles prepared in Example 2 of the present invention;
[0030] Figure 3 Transmission electron microscopy (TEM) image of the barium titanate ultrafine piezoelectric nanoparticles prepared in Example 3 of this invention;
[0031] Figure 4 Transmission electron microscope image of lithium niobate ultrafine piezoelectric nanoparticles prepared in Comparative Example 1 of this invention;
[0032] Figure 5 The X-ray diffraction pattern of the lithium niobate ultrafine piezoelectric nanoparticles prepared in Example 1 of this invention;
[0033] Figure 6 The X-ray diffraction pattern of the lithium tantalate ultrafine piezoelectric nanoparticles prepared in Example 2 of this invention;
[0034] Figure 7 The X-ray diffraction pattern of the barium titanate ultrafine piezoelectric nanoparticles prepared in Example 3 of this invention.
[0035] Figure 8 The X-ray diffraction pattern is shown for the lithium niobate ultrafine piezoelectric nanoparticles prepared in Comparative Example 1 of this invention. Detailed Implementation
[0036] It should be noted that the following detailed description is illustrative and intended to provide further explanation of the invention. Unless otherwise specified, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.
[0037] The present invention will be further described below with reference to the embodiments.
[0038] Example 1
[0039] A method for preparing ultrafine piezoelectric nanoparticles with ultrasound assistance includes the following steps:
[0040] (1) Place the lithium niobate wafer in a ceramic boat;
[0041] (2) Place the ceramic boat containing lithium niobate wafers into a transparent quartz tube, with an air inlet and an air outlet at each end of the quartz tube.
[0042] (3) Secure the ultrasonic transducer tightly to the lower surface of the ceramic boat, turn on the ultrasonic transducer, and use an ultrasonic frequency of 40 kHz and a power of 300 W.
[0043] (4) The upper surface of the lithium niobate wafer in the ceramic boat was ablated using a nanosecond pulsed laser with a wavelength of 1064 nm, and the laser power density was set to 5 J / cm². 2 The processing area is 1cm 2 The processing time is 60 minutes;
[0044] (5) High-purity argon gas is introduced from the inlet end of the quartz tube at a flow rate of 100 mL / min.
[0045] (6) Place the filter membrane at the outlet of the quartz tube to collect lithium niobate ultrafine piezoelectric nanoparticles;
[0046] (7) Place the filter membrane that adsorbs lithium niobate nanoparticles into a centrifuge tube containing anhydrous ethanol and sonicate for 5 min to obtain a suspension of ultrafine piezoelectric lithium niobate nanoparticles.
[0047] (8) After centrifuging the nanoparticle suspension, vacuum dry it for 12 h at a drying temperature of 40 °C to obtain lithium niobate ultrafine piezoelectric nanoparticle powder.
[0048] Example 2
[0049] A method for preparing ultrafine piezoelectric nanoparticles with ultrasound assistance includes the following steps:
[0050] (1) Place lithium tantalate particles with a particle size of 10 μm in a ceramic boat and compact them to obtain a smooth upper surface;
[0051] (2) Place the ceramic boat containing lithium tantalate particles into a transparent quartz tube, with an air inlet and an air outlet at each end of the quartz tube.
[0052] (3) Securely connect the ultrasonic transducer to the lower surface of the ceramic boat, turn on the ultrasonic wave, and use an ultrasonic frequency of 40 kHz and a power of 300 W.
[0053] (4) The lithium tantalate powder inside the ceramic boat was ablated using a nanosecond pulsed laser with a wavelength of 1064 nm, and the laser power density was set to 5 J / cm². 2 The processing area is 1cm 2 The processing time is 60 minutes;
[0054] (5) High-purity argon gas is introduced from the inlet end of the quartz tube at a flow rate of 100 mL / min.
[0055] (6) Place the filter membrane at the gas outlet of the quartz tube to collect lithium tantalate ultrafine piezoelectric nanoparticles;
[0056] (7) Place the filter membrane that adsorbs lithium tantalate nanoparticles into a centrifuge tube containing anhydrous ethanol and sonicate for 5 min to obtain a suspension of ultrafine piezoelectric lithium tantalate nanoparticles.
[0057] (8) After centrifuging the nanoparticle suspension, vacuum dry it for 12 h at a drying temperature of 40 °C to obtain lithium tantalate ultrafine piezoelectric nanoparticle powder.
[0058] Example 3
[0059] A method for preparing ultrafine piezoelectric nanoparticles with ultrasound assistance includes the following steps:
[0060] (1) Place barium titanate particles with a particle size of 20 μm in a ceramic boat and compact them to obtain a smooth upper surface;
[0061] (2) Place the ceramic boat containing barium titanate particles into a transparent quartz tube, with an air inlet and an air outlet at each end of the quartz tube.
[0062] (3) Secure the ultrasonic transducer tightly to the lower surface of the ceramic boat, turn on the ultrasonic transducer, and use an ultrasonic frequency of 40 kHz and a power of 300 W.
[0063] (4) The barium titanate powder inside the ceramic boat was ablated using a nanosecond pulsed laser with a wavelength of 532 nm, and the laser power density was set to 8 J / cm². 2 The processing area is 2cm² 2 The processing time is 40 minutes;
[0064] (5) High-purity argon gas is introduced from the inlet end of the quartz tube at a flow rate of 100 mL / min.
[0065] (6) Place the filter membrane at the outlet of the quartz tube to collect barium titanate ultrafine piezoelectric nanoparticles.
[0066] (7) Place the filter membrane that adsorbs barium titanate nanoparticles into a centrifuge tube containing anhydrous ethanol and sonicate for 5 min to obtain a suspension of barium titanate ultrafine piezoelectric nanoparticles.
[0067] (8) After centrifuging the nanoparticle suspension, vacuum dry it for 12 h at a drying temperature of 40 °C to obtain barium titanate ultrafine piezoelectric nanoparticle powder.
[0068] Comparative Example 1
[0069] The difference from Example 1 is that the ultrasound step is omitted, while everything else is the same as in Example 1.
[0070] Figure 1 , Figure 2 and Figure 3 TEM images of the ultrafine piezoelectric nanoparticle powders obtained in Examples 1, 2, and 3 are described respectively. As can be seen from the figures, the ultrafine piezoelectric nanoparticles obtained in Examples 1-3 have a particle size in the range of 5-20 nm, uniform particle size distribution, high sphericity, and no obvious agglomeration. Figure 4 TEM images of the piezoelectric nanoparticle powder obtained in Comparative Example 1 are described. The particle size is unevenly distributed in the range of 5-50 nm, and some particles are irregular in shape and larger than the particles obtained under ultrasonic conditions.
[0071] Figure 5 , Figure 6 and Figure 7 XRD images of the ultrafine piezoelectric nanoparticle powders obtained in Examples 1, 2, and 3 are described respectively. As shown in the figures, the composition of the ultrafine piezoelectric nanoparticles obtained in Examples 1-3 conforms to the LiNbO3, LiTaO3, and BaTiO3 phases, respectively, consistent with the target composition. Furthermore, the obtained ultrafine piezoelectric nanoparticles exhibit high crystallinity, with crystallinities of 90.6%, 89.7%, and 91.3% for LiNbO3, LiTaO3, and BaTiO3 nanoparticles, respectively. Figure 8 The XRD image of the piezoelectric nanoparticle powder obtained in Comparative Example 1 is described. The particle composition is the same as that of the powder obtained under ultrasonic conditions, which conforms to the LiNbO3 phase, but the crystallinity is reduced to 80.6%.
[0072] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for preparing ultrafine piezoelectric nanoparticles using ultrasound-assisted laser, characterized in that: The steps include: placing a ceramic boat containing piezoelectric material raw materials into a quartz tube with an outlet hole and an air inlet hole; An ultrasonic transducer is fixed to the lower surface of a ceramic boat, and ultrasound is applied to the ceramic boat. The ultrasound produces a discharge effect, a Marangoni effect, and an acoustic cavitation effect on the solution in the laser ablation molten pool, which promotes the sputtering of the laser ablation melt and at the same time promotes the refinement of particle size and uniformity of particle size. Simultaneously, the piezoelectric material raw material is subjected to laser ablation. During the laser ablation process, inert gas is used for purging, and nanoparticles are collected using a filter membrane. After laser ablation, the filter membrane is placed in a solvent for ultrasonic cleaning. The resulting nanoparticle suspension is then centrifuged, dried, and ultrafine piezoelectric nanoparticles are obtained. The piezoelectric material raw material is in block or powder form; The particle size of the ultrafine piezoelectric nanoparticles is 5-20 nm; The piezoelectric material is lithium tantalate, lithium niobate, barium titanate, potassium sodium niobate, zinc oxide, titanium oxide, or aluminum zirconate titanate.
2. The method for preparing ultrafine piezoelectric nanoparticles using ultrasound-assisted laser according to claim 1, characterized in that: During laser ablation, the wavelength of the laser is 355-1064 nm and the pulse width is 0.4-20 ns.
3. The method for preparing ultrafine piezoelectric nanoparticles using ultrasound-assisted laser according to claim 2, characterized in that: The laser power density is 0.5-15.0 J / cm². 2 .
4. The method for preparing ultrafine piezoelectric nanoparticles using ultrasound-assisted laser according to claim 1, characterized in that: The ultrasonic frequency is 20-50 kHz; the ultrasonic power is 10-1000 W.
5. The method for preparing ultrafine piezoelectric nanoparticles using ultrasound-assisted laser according to claim 1, characterized in that: The inert gas is nitrogen or argon.
6. The method for preparing ultrafine piezoelectric nanoparticles using ultrasound-assisted laser according to claim 1, characterized in that: The ultrafine piezoelectric nanoparticles were dried under vacuum at a temperature of 20-50 °C for 6-12 h.
7. The method for preparing ultrafine piezoelectric nanoparticles using ultrasound-assisted laser according to claim 1, characterized in that: The solvent is anhydrous ethanol or deionized water.
8. An ultrafine piezoelectric nanoparticle, characterized in that: It is prepared by any of the preparation methods described in claims 1-7.
Citation Information
Patent Citations
Lithium tantalate nano powder and preparation method thereof
CN101602596A
Method for preparing lithium tantalate nano-powder by adopting solvothermal method
CN103787415A
Method for preparation of lithium tantalate nano-powder by hydrothermal process
CN103833079A
Bismuth / barium titanate heterojunction for enhancing sonodynamic tumor resistance and preparation method thereof
CN113209290A
Laser ablation apparatus and method of preparing nanoparticles using the same
CN1743124A