A preform for HP-RTM and a method for producing the same
By sprinkling sizing powder on the surface of the fiber cloth and heating it to penetrate, a dense, integral preform is formed, which solves the problem of fiber cloth being scattered or deformed under high pressure, achieving high toughness and impact resistance, and expanding the thickness and application range of products.
Patent Information
- Application Number
- CN202211303309.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-24
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-10-24
AI Technical Summary
In existing preforming methods, the fiber cloth is prone to scattering or deformation during high-pressure resin injection, which affects the performance of HP-RTM products.
A setting powder (thermoplastic resin) is sprinkled on the surface of the fiber cloth. The setting powder is melted by heating and penetrates into the fiber gaps to form a dense, integral preform. Thermoplastic resin is used to improve toughness and resistance to high-pressure impact.
The prepared preform is not easily deformed under high pressure, has good toughness and resilience, and can be used to prepare thicker composite material products with a wide range of applications.
Smart Images

Figure CN117962164B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of preforming technology, and in particular to a preform for HP-RTM and its preparation method. Background Technology
[0002] HP-RTM (High Pressure Resin Transfer Molding) is a molding method that uses high pressure to mix resin and inject it into a vacuum-sealed mold pre-laid with fiber reinforcement and inserts. The resin flows through the mold, undergoing impregnation, curing, and demolding to obtain the composite material product. HP-RTM not only shortens the filling time but also maintains the morphology and surface quality of the part, offering unique advantages. Because HP-RTM molding is currently fast and involves high resin injection pressure, the fiber cloth placed in the mold beforehand needs to be pre-formed to pre-shape the product's appearance.
[0003] Existing preforming methods typically involve stacking each sheet of fiber fabric in a preforming mold for compression preforming, and then stacking the preformed fiber fabrics in an HP-RTM device for high-pressure resin injection. Directly stacking multiple fiber fabrics in the HP-RTM device, due to the high pressure used during resin injection, can easily cause the multiple fiber fabrics to disperse or deform, affecting the performance of the HP-RTM product. Summary of the Invention
[0004] Based on the above analysis, the present invention aims to provide a preform for HP-RTM and a method for preparing the same, in order to solve the problem that preforms prepared by existing preforming methods are easily deformed under high pressure.
[0005] On one hand, embodiments of the present invention provide a method for preparing a preform for HP-RTM, such as... Figure 1 As shown, the method includes:
[0006] (1) Sprinkle setting powder on the surface of the fiber cloth, wherein the setting powder is a thermoplastic resin;
[0007] (2) Stack multiple fiber cloths and place them in a pre-forming mold. Heat the fiber cloths to melt the sizing powder on the surface of the fiber cloths. Press the stacked fiber cloths to thin them out and pre-form them, while allowing the molten sizing powder to penetrate into the fiber gaps.
[0008] (3) Cool the product after pressing in step (2) to change the molten shaping powder from liquid to solid, and combine the dispersed fiber cloth into a whole to obtain a preform.
[0009] Preferably, the shaping powder is at least one of polypropylene resin, polyamide resin, polyester resin, polyphenylene ether resin, and polystyrene.
[0010] Preferably, the amount of the setting powder is 8-12 g / m³. 2 .
[0011] Preferably, in step (2), stacking multiple fiber cloths includes: marking the center point of each layer of fiber cloth, marking the middle part of the stacking fixture, overlapping the marking points of the fiber cloth and the marking points of the fixture, and stacking each layer of fiber cloth.
[0012] Preferably, in step (2), the heating temperature is 120-180℃.
[0013] Preferably, in step (2), the pressure applied is 1000KN-5000KN.
[0014] Preferably, in step (2), the heating method is at least one of infrared heating, contact heating and microwave resonant heating.
[0015] Preferably, the method further includes cutting, trimming and punching the preform obtained in step (3).
[0016] On the other hand, the present invention also provides a preform obtained according to the above method.
[0017] Thirdly, the present invention also provides the application of the above-mentioned preform in HP-RTM.
[0018] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0019] 1. This invention involves sprinkling setting powder onto fiber cloth, stacking multiple fiber cloths, and then heating to melt the setting powder. During preforming under pressure, the molten setting powder penetrates into the fiber gaps, resulting in a tightly and uniformly bonded preform of each layer of fiber cloth in the cooled preform. The preform prepared by this invention is a bonded whole, rather than a dispersed stack. When this preform is used in HP-RTM, high-pressure resin is injected from a direction perpendicular to the fiber cloth surface, and the preform will not be scattered or deformed due to high-pressure impact.
[0020] 2. The shaping powder used in this invention is a thermoplastic resin. Thermoplastic resin molecules are cross-linked chains, and after cooling and shaping, they can be softened again by heating and reshaped. Therefore, using thermoplastic resin to shape multi-layer fiber cloth results in a preform with good toughness and resilience. HP-RTM also heats the preform during high-pressure fluid injection. Because the thermoplastic resin remelts upon heating, it prevents the preform from deforming, breaking, or being damaged under the high-pressure fluid impact of HP-RTM. This invention does not use thermosetting resin as a shaping agent because thermosetting resin, after being heated and cooled again, will not remelt upon reheating, exhibiting high brittleness. It is prone to cracking and damage under the high-pressure fluid impact of HP-RTM, leading to deformation of the preform.
[0021] 3. Thermoplastic resins are petroleum derivatives, which are environmentally friendly and cause little pollution to the environment.
[0022] 4. Existing preforms cannot be used to produce products with a thickness exceeding 20 mm because excessive thickness makes them more susceptible to being broken apart by high pressure. However, the preform of this invention has strong resistance to high-pressure impact, and the preform can be thicker, thus enabling the production of products with a thickness ≥ 40 mm.
[0023] 5. This invention cuts the prepared integral preform into multiple blanks, thereby improving the blank production efficiency;
[0024] 6. The preform prepared by the preparation method of the present invention can be used not only for preparing leaf springs by HP-RTM method, but also for preparing battery casings and front covers by HP-RTM method, and has a wide range of applications.
[0025] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained from what is particularly pointed out in the description and drawings. Attached Figure Description
[0026] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.
[0027] Figure 1 This is a flowchart of the method for preparing a preform for HP-RTM according to the present invention.
[0028] Figure 2 This is a longitudinal sectional view of the HP-RTM rapid prototyping mold of the present invention;
[0029] Figure 3This is a schematic cross-sectional view of the HP-RTM rapid prototyping mold of the present invention;
[0030] Figure 4 This is another longitudinal sectional view of the HP-RTM rapid prototyping mold of the present invention;
[0031] Figure 5 This is an enlarged schematic diagram of the sealing structure, encapsulation seal, and gas seal of the HP-RTM rapid prototyping mold vacuum control valve of the present invention;
[0032] Figure 6 This is a physical image of the finished product of Embodiment 6 of the present invention.
[0033] The annotations in the attached figures are explained as follows:
[0034] 100-Upper mold, 101-Upper mold fixing plate, 102-Upper mold pad, 103-Upper mold heat insulation plate, 104-Upper mold core, 105-Upper mold insulation plate, 106-Pressure sensor, 107-Injection port, 108-Upper mold temperature sensor, 109-Guide sleeve, 110-Vacuum system, 111-Air nozzle, 112-Vacuum pipeline, 113-Vacuum cylinder, 114-Vacuum control valve, 1141-O-ring seal, 1142-Valve sleeve, 1143-Valve stem, 115-Vacuum oil circuit 116-Vacuum gauge, 120-Upper mold temperature controller, 200-Lower mold, 201-Lower mold fixing plate, 202-Lower mold pad, 203-Lower mold heat insulation plate, 204-Lower mold core, 205-Lower mold insulation plate, 206-Sealing glue, 207-Air seal, 208-Support block, 209-Guide post, 210-Ejection mechanism, 211-Push plate, 212-Ejector rod, 213-Ejection cylinder, 214-Lower mold temperature sensor, 220-Lower mold temperature controller, 300-Cavity. Detailed Implementation
[0035] Preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which form part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.
[0036] On the one hand, the present invention provides a method for preparing a preform for HP-RTM, such as... Figure 1 As shown, the method includes:
[0037] (1) Sprinkle setting powder on the surface of the fiber cloth, wherein the setting powder is a thermoplastic resin;
[0038] (2) Stack multiple fiber cloths and place them in a pre-forming mold. Heat the fiber cloths to melt the setting powder on the surface of the fiber cloths. Press the stacked fiber cloths to thin them out and pre-form them, while allowing the molten setting powder to penetrate into the fiber gaps.
[0039] (3) Cool the product after pressing in step (2) to change the molten shaping powder from liquid to solid, and combine the dispersed fiber cloth into a whole to obtain a preform.
[0040] Compared with existing technologies, the method provided in this embodiment involves sprinkling setting powder onto fiber cloth, stacking multiple layers of fiber cloth, and then heating to melt the setting powder. During preforming under pressure, the molten setting powder penetrates into the fiber gaps, resulting in a tightly and uniformly bonded preform where each layer of fiber cloth is bonded together. The preform prepared by this invention is a bonded whole, not a dispersed stack. When this preform is used in HP-RTM, high-pressure resin is injected from a direction perpendicular to the fiber cloth surface, and the preform will not be dispersed or deformed due to the high-pressure impact. The setting agent used in this invention is a thermoplastic resin. Thermoplastic resin molecules are chain-crosslinked, and after cooling and setting, they can be softened again by heating and re-set. Therefore, using thermoplastic resin to set multiple layers of fiber cloth results in a preform with good toughness and resilience. HP-RTM also heats the preform during high-pressure fluid injection. Because the thermoplastic resin remelts upon heating, it prevents the preform from deforming, breaking, or being damaged under the high-pressure fluid impact of HP-RTM. This invention does not use thermosetting resin as a setting agent because thermosetting resins, after being heated and cooled again, will not remelt upon reheating, exhibiting high brittleness and easily cracking and being damaged under the high-pressure fluid impact of HP-RTM, leading to preform deformation. Furthermore, thermoplastic resin is a petroleum derivative, making it environmentally friendly with minimal pollution. Existing preforms are no thicker than 20mm because excessive thickness makes them more susceptible to being broken apart by high pressure. The preform of this invention has strong resistance to high-pressure impact, allowing for greater thickness, thus enabling the production of products with a thickness ≥40mm.
[0041] In step (1) of the present invention, a powder spraying machine can be used to spray the setting powder evenly on the surface of the fiber cloth.
[0042] In this invention, powder can first be sprayed onto a continuous sheet of fiber cloth. After powdering, the fiber cloth can then be cut, perforated, or spliced using a cutting machine according to product dimensions and mold requirements. Figure 1 As shown.
[0043] In this invention, the specific selection of the setting agent can be made by comprehensively considering the setting effect and the performance of the high-pressure fluid in the subsequent HP-RTM. Preferably, the setting agent has good setting properties, high compatibility with the high-pressure fluid in HP-RTM, and does not chemically react with the high-pressure fluid.
[0044] For example, the setting powder is at least one selected from polypropylene resin, polyamide resin, polyester resin, polyphenylene ether resin, and polystyrene. The setting powder may also be a modified version of the above substances.
[0045] In this invention, to further improve the setting effect of the setting agent and its resistance to high-pressure fluid impact, the amount of setting powder used is 8-12 g / m³. 2 For example, 9g / m 2 10g / m 2 11g / m 2 .
[0046] In this invention, to ensure that multiple fiber fabrics are stacked neatly, step (2) involves stacking the multiple fiber fabrics by: marking the center point of each layer of fiber fabric and also marking the center of the stacking fixture; overlapping the markings on the fiber fabric and the fixture; and stacking the layers of fiber fabric. Using the center markings prevents the multiple fiber fabrics from becoming scattered.
[0047] For example, the fiber cloth is at least one of glass fiber, carbon fiber, basalt fiber, aramid fiber, and plant fiber.
[0048] For example, the fiber cloth is woven in at least one of the following methods: unidirectional cloth, checkered cloth, mesh cloth, warp-knitted cloth, and axial cloth.
[0049] In step (2) of the present invention, the heating is used to melt the sizing powder, allow it to penetrate and flow in the fiber cloth, and the heating temperature can be determined according to the melting temperature of the sizing powder.
[0050] For example, in step (2), the heating temperature is 120-180°C.
[0051] For example, in step (2), the heating method is at least one of infrared heating, contact heating and microwave resonant heating.
[0052] In step (2) of the present invention, the function of applying pressure is to make the molten shaping powder penetrate more evenly into the fiber gaps while the fiber cloth is pre-formed.
[0053] For example, in step (2), the pressure applied is 1000KN-5000KN.
[0054] In step (3) of the present invention, the cooling function is to remove the heat from the preform. As the temperature decreases, the sizing powder changes from liquid to solid and solidifies in the fiber cloth, thereby tightly connecting the different layers of fiber cloth together, so that the originally dispersed fiber cloth is combined into a whole, which can avoid the displacement and damage to the preform caused by high pressure impact.
[0055] For example, the cooling method is to introduce cooling liquid into the preform mold to remove the heat from the preform.
[0056] For example, the method further includes cutting, trimming and punching the preform obtained in step (3).
[0057] For example, the thickness of the preform of the present invention is ≥40mm.
[0058] For example, the preform cutting method is one or more of vibration cutting, laser cutting, ultrasonic cutting, and high-pressure water cutting. More preferably, the cutting method is ultrasonic cutting. Ultrasonic cutting is more suitable for cutting thicker preforms.
[0059] Specifically, the conditions for using ultrasonic cutting in blank cutting are: air supply pressure 6-8 bar, amplitude 37-42%, and cutting speed 20-60 mm / s.
[0060] Ultrasonic cutting technology involves converting electric current into electrical energy using an ultrasonic generator. This high-frequency electrical energy is then converted into mechanical vibrations of the same frequency by a transducer. These mechanical vibrations are then transmitted to the cutting blade via an amplitude modulator. The cutting blade transfers the received vibrational energy to the cutting surface of the workpiece, thus cutting the blank.
[0061] An air supply pressure of 6-8 bar ensures sufficient air volume, allowing the cutter to cool down promptly and extend its service life. An amplitude of 37-42% ensures effective cutting of the blank without damaging the cutter due to excessive vibration. A cutting speed of 20-60 mm / s guarantees a smooth, secure cut, accurate edges, and prevents deformation, warping, fraying, stringing, or wrinkling. Furthermore, maintaining a 90° angle between the cutter tip and the ground, and keeping the cutting path parallel to the outer edge of the mold, minimizes shape errors in the blank during cutting, resulting in a complete, high-quality blank.
[0062] This invention uses an ultrasonic cutting blade. By optimizing the blade's amplitude, speed, cutting angle, and path, it can quickly and efficiently cut out complete, high-quality blanks, improving efficiency. Combined with pre-forming process steps, it can produce products with complex structures and a thickness of ≥40mm.
[0063] Specifically, the pressed preform is placed on a cutting fixture and secured with bolts. Based on the actual dimensions and redundancy of the preform, it is then cut, trimmed, and drilled.
[0064] Cutting the preformed blank into multiple blanks improves the efficiency of blank production.
[0065] Secondly, the present invention also provides a preform obtained by the above method.
[0066] The preform is a bonded whole, not a discrete stack. It exhibits strong impact resistance. The preform can be thicker, allowing for the production of products with a thickness ≥40mm. Furthermore, the shaping powder in the preform is a thermoplastic resin, resulting in good overall toughness, resilience, and shape retention.
[0067] Thirdly, the present invention also provides the application of the above-mentioned preform in HP-RTM.
[0068] When the preform is applied to HP-RTM, high-pressure resin is injected from a direction perpendicular to the surface of the fiber cloth. The preform will not be broken or deformed due to the high-pressure impact. During the high-pressure injection of fluid in HP-RTM, there is a heating process. Since the thermoplastic resin will melt again when heated, the preform can be prevented from deforming, breaking or being damaged under the high-pressure fluid impact of HP-RTM.
[0069] The present invention also provides a rapid prototyping mold for composite material components in HP-RTM, which is used to realize the application of the above-mentioned preform in HP-RTM, that is, when the above-mentioned preform is applied in HP-RTM, the mold is used.
[0070] A composite material component HP-RTM rapid prototyping mold includes: an upper mold 100, a lower mold 200, a vacuum system 110, a sealing structure 206, an airtight structure 207, a temperature control system, and a pressure control system, wherein the upper mold 100 and the lower mold 200 form a cavity 300.
[0071] The upper mold 100 is provided with a vacuum control valve mounting port, and the cavity 300 is connected to the vacuum system 110 through the vacuum control valve 114 in the vacuum control valve mounting port.
[0072] The vacuum control valve 114 is equipped with a high-temperature resistant O-ring 1141 and a conical mechanical seal structure.
[0073] Specifically, the vacuum control valve includes a valve stem 1143 and a valve sleeve 1142, which form a conical mechanical seal structure.
[0074] In one possible implementation, the valve stem 1143 includes a first equal-diameter segment, a curved segment, and a second equal-diameter segment connected sequentially. The inner wall of the valve sleeve 1142 includes a first equal-diameter segment, a curved segment, and a second equal-diameter segment whose diameters decrease sequentially and are connected sequentially. The valve sleeve 1142 is fitted onto the valve stem 1143, with a clearance fit between the first equal-diameter segment of the valve stem 1143 and the first equal-diameter segment of the inner wall of the valve sleeve 1142, a transition fit between the curved segment of the valve stem 1143 and the curved segment of the inner wall of the valve sleeve 1142, and a transition fit between the second equal-diameter segment of the valve stem 1143 and the second equal-diameter segment of the inner wall of the valve sleeve 1142.
[0075] In this invention, after the mold is closed and pressurized, a vacuum needs to be drawn. The cavity 300 is connected to the vacuum system 110 through the vacuum control valve 114 in the vacuum control valve mounting port. To facilitate vacuuming, the gap at the end of the cavity is smaller than the gap in the middle of the cavity along the resin flow direction. The cavity end of the vacuum control valve has a horizontal opening end. Compared with the cavity end part at its front end, this horizontal opening end is provided with an expansion section to facilitate the flow of vacuum air, improve vacuuming efficiency, and obtain a higher vacuum rate.
[0076] The vacuum control valve mounting port is located in the upper mold 100, within the horizontal mating section area at the end of the cavity 300 of the upper mold 100 and lower mold 200. Considering that the cavity 300 has a preform accommodating space and provides a resin flow filling space, the HP-RTM process has a large mold closing clearance and a high injection pressure, and the low-viscosity resin used has the characteristic of fast injection flow rate, in order to achieve vacuuming while effectively controlling the speed of pressurized resin injection and minimizing the possibility of resin entering the vacuum control valve, the horizontal length of the horizontal opening end at the cavity end is greater than the wall thickness of the second equal diameter section of the valve sleeve 1142, but less than the sum of the wall thickness of the second equal diameter section of the valve sleeve 1142 and the diameter of the second equal diameter section of the valve stem 1143. The mating clearance between the valve sleeve 1142 and the valve stem 1143 is not completely located within the horizontal area of the horizontal opening end at the cavity end.
[0077] Since the fitting clearance between the valve sleeve 1142 and the valve stem 1143 is located in the horizontal region of the horizontal opening at the end of the cavity, in order to further prevent resin from entering the vacuum control valve and causing blockage of the mold injection port and vacuum port, resulting in damage to the mold sealing structure, the vacuum control valve of the present invention also includes a high-temperature resistant O-ring.
[0078] The number of high-temperature resistant O-rings is multiple. In one possible embodiment, three sets of high-temperature resistant O-rings 1141 are provided on the mating surfaces of the valve sleeve 1142 and the valve stem 1143. The first and second sets of high-temperature resistant O-rings 1141 are located on the second equal diameter section of the valve stem 1143 and the second equal diameter section of the inner wall of the valve sleeve 1142. The third set of high-temperature resistant O-rings 1141 is located on the curved section of the valve stem 1143 and the curved section of the inner wall of the valve sleeve 1142.
[0079] Specifically, sealing ring mounting grooves are respectively opened on the first equal diameter section, the curved section and the second equal diameter section of the valve stem 1143, and high temperature resistant O-rings are installed in the sealing ring mounting grooves.
[0080] Since the cavity is formed by the mating of an upper mold and a lower mold, to facilitate vacuuming, one side wall of the vacuum control valve mounting port is flush with the edge of the horizontal opening at the end of the cavity, and the valve sleeve 1142 is fitted with the upper mold core 104 of the upper mold. To prevent resin from entering the mating surface between the valve sleeve 1142 and the upper mold core 104, a high-temperature resistant O-ring 1141 is provided between the valve sleeve 1142 and the upper mold core 104. A sealing ring mounting groove is provided on the outer surface of the valve sleeve 1142, and the high-temperature resistant O-ring 1141 is installed in the sealing ring mounting groove.
[0081] The present invention is provided with four sets of high-temperature resistant O-rings 1141. Three sets of high-temperature resistant O-rings are sequentially sleeved on the valve stem 1143 along the axial direction of the valve stem 1143. The first and second sets of high-temperature resistant O-rings 1141 are located on the cylindrical mating surface of the second equal diameter section, and the third set of high-temperature resistant O-rings 1141 is located on the conical mating surface of the curved section. The fourth set is located on the mating surface between the valve sleeve 1142 and the upper mold core 104 of the upper mold.
[0082] To further improve sealing performance, the spacing between the first, second, and third sets of high-temperature O-rings gradually increases along the axial direction of valve stem 1143. The fourth set of high-temperature O-rings is located between the second and third sets of high-temperature O-rings, and the second and fourth sets of high-temperature O-rings partially overlap in the axial direction.
[0083] To further improve sealing performance, the spacing between the first, second, and third sets of high-temperature resistant O-rings is as follows: The first set of high-temperature resistant O-rings is positioned on the cylindrical mating surface of the second equal-diameter section of the valve stem 1143, at half the length of the second equal-diameter section from bottom to top (the measurement reference is the length of the second equal-diameter section of the valve stem 1143, with the starting point being the lower end face). The second set of high-temperature resistant O-rings is positioned on the cylindrical mating surface of the second equal-diameter section of the valve stem 1143, starting from bottom to top... At 3 / 4 of the length of the second equal-diameter segment (measurement reference is the length of the second equal-diameter segment of valve stem 1143, starting from the lower end face), the third set of high-temperature resistant O-rings 1141 is located on the tapered mating surface of valve stem 1143. At 1 / 2 of the sum of the lengths of the curved segment and the second equal-diameter segment of valve stem 1143 (measurement reference is the sum of the lengths of the curved segment and the second equal-diameter segment of valve stem 1143, starting from the lower end face), the fourth set of high-temperature resistant O-rings is located on the mating surface between valve sleeve 1142 and upper mold core 104 of upper mold. The dimensions of the first, second, third, and fourth sets of high-temperature resistant O-rings meet the standardization requirements.
[0084] Through the above structural design, the mold sealing structure is not easily damaged in the molding cycle production of the present invention, thereby avoiding vacuum failure and effectively extending the life cycle of the mold.
[0085] Compared with existing molds, this invention uses a metal mechanical seal and a high-temperature resistant sealing ring to seal the vacuum control valve, which effectively extends the mold life cycle and reduces the number of mold repairs in mass production.
[0086] It should be noted that, due to the unique characteristics of the HP-RTM molding process, the lifespan of the mold sealing structure directly affects the mold's cycle life. The resin is liquid before curing and solid after curing. In actual production, existing sealing structures are prone to damage to the sealing rings or resin adhesion to the mechanical seal. In subsequent production cycles, this can easily lead to vacuum system failure, causing the entire vacuum system to become filled with resin, resulting in irreversible damage to the mold and equipment. To address these issues, four sets of high-temperature resistant O-rings and conical mechanical seals are installed at the vacuum control valve from bottom to top. Each sealing structure functions to isolate the resin and provide a seal, effectively preventing resin overflow and air leakage. Even if one set of seals fails, the subsequent sets will remain effective, allowing the production cycle to continue uninterrupted, effectively extending the mold's lifespan.
[0087] Specifically, the sealing structure 206 is located on the parting surface of the lower mold core 104 and is situated outside the cavity. The air seal structure 207 is located outside the sealing structure 206, near the edge of the mold, specifically on the outer side of the horizontal opening end of the cavity. The sealing structure 206 and the air seal structure 207 are sequentially arranged thereon.
[0088] Specifically, the ends of the upper mold 100 and the lower mold 200 are fitted together by steps, and the air seal 207 structure is located at the mating surface of the upper mold 100 and the lower mold 200.
[0089] The sealing structure achieves a vacuum effect, and the airtight structure can effectively form a secondary sealed space, making the entire cavity 300 space more reliable.
[0090] Furthermore, the upper mold 100 includes an upper mold fixing plate 101, an upper mold pad 102, an upper mold heat insulation plate 103, an upper mold core 104, an upper mold insulation plate 105, an injection port 107, and a guide sleeve 109.
[0091] The upper mold pad 102 is connected to the upper mold fixing plate 101, and the upper mold core 104 is connected to the other side of the upper mold pad 102. An upper mold heat insulation plate 103 is installed between the upper mold core 104 and the upper mold pad 102. An upper mold insulation plate 105 covers the periphery of the upper mold core 104. The injection port 107 is connected to the upper mold core 104, with its bottom surface flush with the lower surface of the upper mold core 104. The guide sleeve 109 is connected to the upper mold core 104 and is concentric with the guide post 209. The gap between the injection port 107 and the injection nozzle of the HP-RTM high-pressure injection molding equipment is sealed by a high-temperature resistant O-ring.
[0092] Furthermore, the lower mold 200 includes a lower mold fixing plate 201, a lower mold pad 202, a lower mold heat insulation plate 203, a lower mold core 204, a lower mold insulation plate 205, a support block 208, and a guide post 209.
[0093] The lower mold pad 202 is connected to the lower mold fixing plate 201. The other end of the lower mold pad 202 is connected to the lower mold core 204. The lower mold heat insulation plate 203 is installed between the lower mold pad 202 and the lower mold core 204. The lower mold insulation plate 205 is connected to the lower mold core 204 and covers the outside of the lower mold core 204. The support block 208 is connected to the upper end face of the lower mold core 204. The guide post 209 is connected to the upper end face of the lower mold core 204 and is concentric with the guide sleeve 109.
[0094] Specifically, the temperature control system includes an upper mold temperature control system and a lower mold temperature control system; the upper mold temperature control system includes an upper mold temperature controller 120 and an upper mold temperature sensor 108.
[0095] Specifically, the mold also includes a pressure control system, which includes a pressure sensor 106.
[0096] Specifically, the upper mold core 104 has a length of 'a', and the upper mold temperature sensor 108 is connected to the side of the upper mold core 104 and is disposed on the upper mold core. place, place, The upper mold temperature controller 120 is located inside the upper mold core 104 and is connected to the side of the upper mold core 104.
[0097] Specifically, the lower mold core 204 has the same length as the upper mold core 104, and the lower mold temperature sensor 214 is connected to the outside of the lower mold core 204 and is disposed on the lower mold core. place, place, The lower mold temperature controller 220 is located inside the lower mold core 204 and is connected to the outside of the lower mold core 204.
[0098] Specifically, pressure sensors 106 are respectively disposed at the connection points of the upper mold core 104 and the cavity 300. The pressure sensors 106 are connected to the upper mold core 104 and are flush with the upper surface of the cavity 300.
[0099] The temperature and pressure control systems can effectively provide feedback on pressure changes and mold temperature changes during the entire injection molding process of thermosetting resin. By combining this data with the overall quality data of the prototype parts, the injection pressure and mold temperature can be adjusted, effectively reducing the trial production cycle of qualified prototype parts and lowering the production cost of the product.
[0100] Specifically, the lower mold 200 includes an ejection mechanism 210, which consists of a push plate 211, an ejector rod 212, and an ejection cylinder 213. The ejector rod 212 is provided with a high-temperature resistant O-ring seal, and there are two sets of high-temperature resistant O-ring seals, which are arranged sequentially below the ejection height of the ejector rod.
[0101] To ensure synchronized and automatic ejection of the resin product, the number and position of the ejector pins need to meet certain conditions. Specifically, there are four ejector pins 212, each positioned in the lower mold core. place, place, place, At the location, the push rod 212 is connected and fixed to the push plate 211. Each of the four ends of the push plate 211 is provided with an ejection cylinder 213. One end of the ejection cylinder 213 is connected and fixed to the push plate 211, and the other end of the ejection cylinder 213 is connected and fixed to the lower mold fixing plate 201. The oil circuits of the four ejection cylinders 213 are connected in series.
[0102] It should be noted that when the ejector cylinder 213 ejects, the ejector rod 212 will be ejected simultaneously, thereby ensuring the product is ejected smoothly. This avoids damage to the product's shape due to asynchronous ejection of the ejector rod 212, or the product being ejected at one end while the other end is stuck in the cavity 300. The synchronous ejection of the ejector rod 212 makes the production process more stable and reliable, and reduces the defect rate.
[0103] Composite material components prepared by the HP-RTM rapid prototyping mold provided by this invention have a shorter molding cycle, higher molding efficiency, lower manufacturing cost, and smooth double-sided products. At the same time, by using the preform of this invention, products with a thickness of ≥40mm can be prepared.
[0104] The preform of the present invention can be used not only for preparing leaf springs by HP-RTM method, but also for preparing battery casings and front covers by HP-RTM method, and has a wide range of applications.
[0105] The following specific embodiments further illustrate the preform for HP-RTM and its preparation method of the present invention.
[0106] Example 1
[0107] A method for preparing a preform for HP-RTM leaf spring fabrication includes:
[0108] HP-RTM composite leaf spring preform
[0109] Based on the layup design results, unidirectional glass fiber cloth and carbon fiber cloth were selected to fabricate the leaf spring preform.
[0110] 1. Apply the sizing powder (modified polypropylene resin) compatible with the epoxy resin at a ratio of 9 g / m³. 2 The amount of product is sprayed onto the surface of glass fiber unidirectional cloth and carbon fiber cloth;
[0111] 2. Place the fiberglass cloth sprinkled with setting powder on the cutting machine for cutting. The cutting size is 1300mm*340mm. Cut a total of 20 layers of fiberglass unidirectional cloth of the same size. Cut 2 layers of carbon fiber unidirectional cloth of 650mm*340mm (mark the midpoint of each layer of carbon fiber cloth) for later use.
[0112] 3. First, place 10 layers of cut unidirectional fiberglass fabric on the stacking fixture, aligning the midpoint of the fabric with the midpoint of the fixture, and aligning all four sides of each fabric layer. Place two layers of carbon fiber fabric on top of the 10 layers of unidirectional fiberglass fabric, ensuring that the midpoints of all fabric layers are aligned with the midpoint of the fixture, and the long side of the carbon fiber fabric is aligned with the long side of the fiberglass fabric. Then place another 10 layers of fiberglass fabric, aligning the midpoint of the fabric with the midpoint of the fixture, and aligning all four sides with the fiberglass fabric placed at the bottom layer.
[0113] 4. Place the laminated carbon fiber / glass fiber cloth into the preforming mold, set the mold temperature to 150℃, set the pressure to 5000KN, and press the thickness to 40mm. After pressing for 20 minutes, start cooling. After the temperature drops to 80℃, turn on the press and take out the preform.
[0114] 5. Place the removed preform on the cutting fixture, clamp the preform using a two-stage fastening method, and then use an ultrasonic cutting device with an air supply pressure of 6 bar, an amplitude of 40%, a cutting speed of 20 mm / s, a cutting power of 200 W, and a cutting frequency of 20000 HZ to cut the preform into preforms with a width of 70 mm each. Trim and punch holes in the preforms.
[0115] Example 2
[0116] A method for preparing a preform for HP-RTM battery casing fabrication includes:
[0117] 1. Add the setting powder (modified polypropylene resin) at a ratio of 11 g / m 2 The amount used is sprayed onto the surface of glass fiber and carbon fiber cloth;
[0118] 2. Using a cutting machine, cut the fiberglass cloth into square pieces of 1200mm*900mm. At the right angle of the cloth, cut 80mm inward at each of the four corners using a 45° angle cutting method, cutting a total of 4 layers; cut one layer of 800mm*800m carbon fiber axial cloth.
[0119] 3. Using a clamping fixture, stack the five layers of fabric together in the order of (glass fiber / glass fiber / carbon fiber / glass fiber / glass fiber), using a stacking fixture and center point alignment method, with the carbon fiber fabric placed in the exact center of the glass fiber fabric.
[0120] 4. Place the five-layer fiber cloth in the pre-forming mold using a clamping device, heat the pre-forming mold to 140℃, keep it at that temperature for 30 minutes, and apply a pressure of 3000KN.
[0121] 5. After the heat preservation is completed, take out the preformed blank and place it on the surface of the cutting fixture. Use a 500HZ vibrating tungsten carbide knife to cut around the blank and remove the flash outside the fixture. Use the vibrating tungsten carbide knife to cut and punch holes on the protruding parts on the upper surface of the blank. After removing the excess parts, keep them for later use.
[0122] Example 3
[0123] A method for preparing a preform for HP-RTM front hood fabrication includes:
[0124] 1. Based on environmental protection and design requirements, basalt fiber warp-knitted fabric and bamboo fiber unidirectional fabric were selected as the main woven fabrics. A powder-spraying machine was used to apply the setting powder (modified polyamide resin) at a rate of 12g / m³. 2 Sprinkle the amount evenly on the surface of the fiber cloth;
[0125] 2. Using a fiber cloth cutting machine, basalt fiber warp-knitted fabric is cut into a semi-circular arc structure of 1000mm*600mm, with a total of 6 layers cut; bamboo fiber checkered fabric is cut into strips of 1000mm*50mm, with a total of 4 layers cut.
[0126] 3. Use stacking fixtures. First, place 3 layers of basalt fiber cloth, then place 4 layers of bamboo fiber cloth at the bottom edge of the basalt fiber cloth, and then place 3 more layers of basalt fiber cloth.
[0127] 4. Place the stacked fiber cloth in a large microwave heating box for microwave heating treatment. Heat at 20000W power for 5 minutes, with a final temperature of 160℃. Quickly transfer it to the machine cover pre-forming mold, press it into a pre-formed blank (rough blank), and cool it.
[0128] 5. Transfer the pressed preform to the cutting fixture and use laser cutting. Set the laser cutting power to 10KW and the cutting speed to 10m / min to remove the excess flash and excess parts of the preform.
[0129] Example 4
[0130] The preform was prepared according to the method in Example 1, except that the amount of shaping powder used was 2 g / m². 2 .
[0131] Example 5
[0132] The preform was prepared according to the method of Example 1, except that the pressure applied was 900 kN.
[0133] Comparative Example 1
[0134] The preform was prepared according to the method of Example 1, except that a thermosetting resin (epoxy resin) was used instead of a thermoplastic resin (polypropylene resin).
[0135] Test case
[0136] HP-RTM molding was performed using the preforms from Examples 1-5 and Comparative Example 1. The results are shown in Table 1.
[0137] Table 1
[0138]
[0139]
[0140] A comparison of the results of Example 1 and Comparative Example 1 shows that the preform using thermoplastic setting powder has a better setting effect; Examples 1-3 show that the preparation method of the present invention is applicable to the preparation of preforms in multiple fields and has a wide range of applications; A comparison of Example 1 and Examples 4-5 shows that by using the amount of setting powder and the pressure applied according to the present invention, a preform with a better setting effect can be obtained.
[0141] Example 6
[0142] A rapid prototyping method for composite material components using HP-RTM (High-Performance-Time Molding) is provided for fabricating composite material leaf springs. The process includes the following steps:
[0143] (1) The required amount of resin was calculated to be 2100g through simulation. The pressure of each component in the dispensing head was adjusted to 140bar. The HUNTSMAN 3585 epoxy resin, HUNTSMAN 3831 amine curing agent and internal release agent were preheated and vacuum degassed. The resin temperature was 80℃, the curing agent temperature was 40℃ and the internal release agent temperature was 28℃. The mixer was adjusted to a low flow circulation mode.
[0144] (2) Clean the impurities on the mold surface, start the press, and open the mold; apply CLE-705 external release agent evenly to the mold surface in small amounts multiple times, with each application being 15ml; heat the mold to 90℃.
[0145] (3) The leaf spring preform was prepared according to the method of Example 1. The difference was that carbon fiber cloth was used. The cut fiber cloth had 34 layers, with a single layer thickness of 1.2 mm. The thickness of the preform was 40 mm. The ultrasonic cutting air supply pressure was 0.65 MPa, the amplitude was 42%, the cutting speed was 20 mm / s, the blade tip was always kept at 90° to the ground, and the cutting path was always kept parallel to the outer edge of the mold. The cut preform was then transferred to the forming mold.
[0146] (4) After the press mold is closed and locked, apply a clamping force of 9000kN;
[0147] (5) Open the vacuum control valve and evacuate for 5 minutes;
[0148] (6) After vacuuming is completed, close the vacuum control valve. Adjust the mixer to high-pressure circulation mode, mix HUNTSMAN3585 epoxy resin, HUNTSMAN 3831 amine curing agent and QZ12-IRA release agent at a mass ratio of 100:24:0.5 until uniform, and then inject the mixture into the fiber cloth in the mold through the injection head installed in the mold at the set injection flow rate of 70g / s and injection time of 30s;
[0149] (7) Hold pressure and cure for 5 minutes to allow the resin to cure and form quickly; after the curing process is completed, release the pressure, open the vacuum control valve to break the vacuum environment, and open the mold; after opening the mold, take out the product, cool it and remove the flash to obtain a composite material leaf spring component with a thickness of 40mm.
[0150] Table 2 Comparison of molding data of Embodiment 6 of the present invention with existing processes.
[0151] project Example 6 Existing prepreg molding technology Single-piece production cycle 20min 120min Molding efficiency high Low Product Costs Leaf spring component: 120 yuan / piece Leaf spring component: 400 yuan / piece Product thickness 40mm ≤20mm
[0152] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. An application of a preform in HP-RTM, characterized in that, The method for preparing the preform includes the following steps: (1) 8~12 g / m 2 A setting powder is sprinkled on the surface of the fiber cloth; the setting powder is a thermoplastic resin. (2) Mark the midpoint of each layer of fiber cloth and the middle part of the stacked tooling. Overlap the markings on the fiber cloth and the tooling. Stack the fiber cloth layers and place them in the pre-forming mold. Heat the fiber cloth at 120-180 ℃ to melt the setting powder on the surface of the fiber cloth, which then penetrates and flows in the fiber cloth. Press the stacked fiber cloth to 1000-5000 kN to thin and pre-form the fiber cloth while allowing the molten setting powder to penetrate into the fiber gaps. (3) Cool the product after pressing in step (2) so that the molten shaping powder changes from liquid to solid and solidifies in the fiber cloth, combining the dispersed fiber cloth into a whole to obtain a preform with a thickness ≥40 mm. (4) Cut, trim and drill holes in the preform obtained in step (3); the preform is cut by ultrasonic cutting, and the conditions for ultrasonic cutting are: air supply pressure 6-8 bar, amplitude 37%-42%, cutting speed 20-60 mm / s; during cutting, the blade tip is kept at 90° to the ground and the cutting path is kept parallel to the outer edge of the mold; cut the preform into multiple blanks; HP-RTM rapid prototyping mold is used for molding. The upper mold is equipped with a vacuum control valve mounting port. The cavity is connected to the vacuum system through the vacuum control valve in the vacuum control valve mounting port. The vacuum control valve includes a valve stem and a valve sleeve, which form a conical mechanical seal structure. The cavity end gap along the resin flow direction is smaller than the cavity middle gap. The cavity end of one end of the vacuum control valve has a horizontal opening end. Compared with the cavity end part at its front end, this horizontal opening end is provided with an expansion section. The horizontal length of the horizontal opening end of the cavity end is greater than the wall thickness of the second equal diameter section of the valve sleeve, but less than the sum of the wall thickness of the second equal diameter section of the valve sleeve and the diameter of the second equal diameter section of the valve stem. The first set of high-temperature resistant O-rings is located on the cylindrical mating surface of the second equal-diameter section of the valve stem, at 1 / 2 of the length of the second equal-diameter section from bottom to top; the second set of high-temperature resistant O-rings is located on the cylindrical mating surface of the second equal-diameter section of the valve stem, at 3 / 4 of the length of the second equal-diameter section from bottom to top; the third set of high-temperature resistant O-rings is located on the tapered mating surface of the valve stem, at 1 / 2 of the sum of the length of the curved section of the valve stem and the second equal-diameter section from bottom to top; the fourth set of high-temperature resistant O-rings is located on the mating surface between the valve sleeve and the upper mold. The sealing structure is located on the parting surface of the lower mold core and outside the cavity; the air-tight structure is located outside the sealing structure.
2. The application according to claim 1, characterized in that, In step (1), the shaping powder is at least one of polypropylene resin, polyamide resin, polyester resin, polyphenylene ether resin, and polystyrene.
3. The application according to claim 1, characterized in that, The amount of the setting powder used is 9-11 g / m 2 .
4. The application according to claim 1, characterized in that, In step (2), the heating method is at least one of infrared heating, contact heating and microwave resonant heating.
Citation Information
Patent Citations
HP-RTM (High Pressure Resin Transfer Molding) rapid forming method and mold for composite material component
CN117621489A
Process of producing preform
JP2011168009A