MOR molecular sieve, preparation method therefor and use thereof

By using inexpensive dimethyldiethylammonium ions as a directing agent, nanosheet-like MOR molecular sieves were synthesized, solving the problems of high preparation cost and complex process in existing technologies, and realizing efficient and economical preparation and application of nanosheet-like MOR molecular sieves.

CN117963938BActive Publication Date: 2026-11-24CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202211313759.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-25
Publication Date
2026-11-24
Estimated Expiration
2042-10-25

AI Technical Summary

Technical Problem

Existing methods for preparing nanoscale MOR molecular sieves typically use expensive organic structure-directing agents or involve complex steps, and the aluminum content is difficult to control, resulting in high costs and cumbersome processes.

Method used

Using inexpensive dimethyldiethylammonium ions as organic structure directing agents, nanosheet-like MOR molecular sieves were directly synthesized through specific raw material ratios and synergistic effects of aluminum sources. The aluminum content was high at the T3 site of the eight-membered ring in the framework, and the preparation method was simple and yielded high.

Benefits of technology

A low-cost, high-yield preparation of nanosheet-shaped MOR molecular sieves was achieved, which have abundant acidity and strong acidity, making them suitable as adsorbents or catalysts for the conversion of organic compounds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117963938B_ABST
    Figure CN117963938B_ABST
Patent Text Reader

Abstract

This invention discloses a MOR molecular sieve, its preparation method, and its applications. The aluminum content at the T3 site of the eight-membered ring in the framework of this invention's MOR molecular sieve is higher than 65% of the total aluminum mass content. It possesses unique aluminum placement sites and a nanosheet morphology. The overall preparation method is simple, low-cost, and has a high yield. The molecular sieve has a high acid content, including many strong acids, and can be used as an adsorbent or a catalyst for the conversion of organic compounds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of molecular sieves, specifically to a MOR molecular sieve, its preparation method, and its applications. Background Technology

[0002] The basic framework structure of crystalline microporous molecular sieves is based on a rigid three-dimensional TO4 (SiO4, AlO4, etc.) unit structure. In this structure, TO4 atoms share oxygen atoms in a tetrahedral manner. The charge balance of the framework tetrahedrons, such as AlO4, is achieved through surface cations, such as Na+. + H + The presence of these pores is maintained. This demonstrates that the framework properties of zeolites can be altered through cation exchange. Furthermore, zeolites possess a rich system of pores with specific pore sizes, which interweave to form a three-dimensional network. Even after the removal of water or organic matter from these pores, the framework remains stable. Based on this structure, molecular sieves not only exhibit excellent catalytic activity and shape selectivity for various organic reactions, but also achieve good selectivity through modification.

[0003] MOR-type molecular sieves have straight channels of eight-membered and twelve-membered rings (0.67 nm × 0.70 nm) along the

[001] direction, and also straight channels of eight-membered rings (0.26 nm × 0.57 nm) along the

[010] direction between the eight-membered and twelve-membered rings. The main channel of MOR molecular sieves is a twelve-membered ring structure, which has good catalytic stability. It has been widely used in processes such as hydrocracking, isomerization, alkylation and reforming, and is also used to separate gas or liquid mixtures. MOR molecular sieves also have extremely high industrial application prospects for dimethyl ether carbonylation reactions.

[0004] Currently, controlling the morphology of MOR molecular sieves is one of the research hotspots. Patent CN1020039C discloses a method for synthesizing high-silica mordenite zeolite, using inexpensive water glass as the silicon source and unalloyed mordenite as the seed crystal to prepare a high-silica mordenite molecular sieve with a silicon-to-aluminum ratio of approximately 25, but the crystal size is larger than 1.0 μm. Patent CN100453461C discloses a method for synthesizing nano-mordenite zeolite molecular sieves, using unalloyed mordenite as the seed crystal and employing a segmented crystallization method to prepare nano-sized mordenite zeolite molecular sieves, but the synthesis steps of this method are relatively complex. Patent CN106698453B discloses a method for synthesizing nano-MOR molecular sieves, firstly by treating the MOR molecular sieve with alkali as a structure directing agent, then mixing the prepared synthetic gel with macroporous carbon, ultrasonically treating it, and then carrying out a crystallization reaction to obtain nano-MOR molecular sieves; this preparation method is also relatively complex. Patent CN102718231B discloses a method for preparing layered nano-mordenite zeolite molecular sieves, using hexadecyltrimethyl-p-methylbenzenesulfonate ammonium salt as an organic structure directing agent. Patent CN107758685B discloses a nano-aggregated sheet-like mordenite zeolite, synthesized by adding a small amount of oxygen-containing organic solvent and the organic structure directing agent tetraethylammonium cation. Patent CN107963637B discloses a method for synthesizing sheet-like nano-mordenite zeolite molecular sieves and the mordenite zeolite molecular sieve itself, using the alkyl monoquaternary ammonium salt hexadecyl N-dimethylethyl-N,N-dimethylammonium bromide as an organic structure directing agent.

[0005] Therefore, current methods for preparing nanoscale MOR molecular sieves typically employ expensive organic structure-directing agents or involve complex and costly preparation steps. Furthermore, the control of aluminum content in the eight-membered rings often relies on post-processing methods, which are cumbersome and difficult to control. Summary of the Invention

[0006] To address the shortcomings of existing technologies, this invention provides a MOR molecular sieve, its preparation method, and its applications. This molecular sieve has unique aluminum sites and a nanosheet morphology. The overall preparation method is simple, low-cost, and has a high yield. The molecular sieve has a large acid content and contains many strong acids, making it suitable as an adsorbent or a catalyst for the conversion of organic compounds.

[0007] The first aspect of the present invention provides a MOR molecular sieve, wherein the aluminum content located at the T3 site of the eight-membered ring in the framework is higher than 65% of the total aluminum mass content.

[0008] Furthermore, the aluminum content at the T3 site of the eight-membered ring in the molecular sieve is 70% to 80% of the total aluminum mass content.

[0009] The molecular sieve has a nanosheet morphology, with an average crystal particle size of no more than 600 nm and an average nanosheet thickness of no more than 30 nm.

[0010] Furthermore, the average crystal size of the molecular sieve is 150–550 nm, and the average thickness of the nanosheets is 15–25 nm.

[0011] Furthermore, in the molecular sieve, plate-like crystals with a thickness of no more than 25 nm account for at least 60% of the total number of crystals, preferably 60% to 90%.

[0012] Furthermore, the aspect ratio of the molecular sieve crystals is preferably 8-35, more preferably 8-20. Unless otherwise specified, the particle size and thickness of the molecular sieve in this invention refer to the average particle size and average thickness, and the aspect ratio is the ratio of the average particle size to the average thickness.

[0013] Furthermore, the silicon-aluminum (SiO2) / Al2O3 molar ratio of the molecular sieve is 18–36.

[0014] Furthermore, the total specific surface area of ​​the molecular sieve is not less than 400 m². 2 / gram, preferably 400-600 meters 2 / gram;

[0015] Furthermore, the external specific surface area of ​​the molecular sieve is not less than 30 m². 2 / gram, preferably 30-100 meters 2 / gram;

[0016] Furthermore, the total pore volume of the molecular sieve is not less than 0.30 cm³. 3 / gram, preferably 0.30 to 0.70 cm 3 / gram;

[0017] Furthermore, the pore volume of the molecular sieve (<2nm) is not less than 0.15 cm³. 3 / gram, preferably 0.15 to 0.25 cm 3 / gram.

[0018] Furthermore, the total acid content of the molecular sieve is not less than 800 μmol / g, preferably 800–1500 μmol / g;

[0019] Furthermore, the molecular sieve has a strong acid content of not less than 300 μmol / g, preferably 300–700 μmol / g.

[0020] A second aspect of the present invention provides a method for preparing MOR molecular sieves, comprising:

[0021] A silicon source, an aluminum source, an alkali source, an organic structure directing agent R, and water are mixed and then crystallized to obtain a MOR molecular sieve.

[0022] The organic structure directing agent R is selected from at least one of dimethyl diethyl ammonium hydroxide, dimethyl diethyl ammonium chloride, dimethyl diethyl ammonium bromide or dimethyl diethyl ammonium iodide, preferably dimethyl diethyl ammonium hydroxide.

[0023] Furthermore, the added silicon source is calculated as SiO2, the aluminum source as Al2O3, and the alkali source as OH. - The organic structure-directing agent R, calculated as dimethyldiethylammonium ions and water, is present in a molar ratio of SiO2:Al2O3:OH. - : R: H2O=1: 0.028~0.056: 0.15~0.38: 0.07~0.17: 10~50.

[0024] Furthermore, the silicon source is silica sol; the aluminum source is sodium aluminate; and the alkali source is sodium hydroxide or potassium hydroxide, preferably sodium hydroxide.

[0025] Furthermore, the sodium aluminate contains 35% to 43% Al2O3 by weight, preferably 38% to 43%, and the sodium aluminate contains 25% to 33% Na2O by weight, preferably 28% to 33%.

[0026] Furthermore, the crystallization treatment conditions include: crystallization at 150–190°C for 0.75–8.0 days, preferably at 160–180°C for 1.0–7.0 days.

[0027] Furthermore, the crystallization process is a dynamic crystallization involving rotation or stirring, with a rotation speed of 10–60 rpm and a stirring speed of 30–300 rpm.

[0028] Furthermore, the yield of the molecular sieve product exceeds 80%, preferably 80% to 95%.

[0029] Furthermore, after the crystallization process, the product can be obtained from the mixture by any conventionally known separation method. Examples of such separation methods include filtering, washing, and drying the obtained mixture. Here, the filtration, washing, and drying can be performed in any manner conventionally known in the art. Specifically, for example, the filtration can be performed by simply vacuum filtering the obtained product mixture. For example, washing can be performed using deionized water and / or ethanol. For example, the drying temperature can be 40–250°C, preferably 60–150°C, and the drying time can be 8–30 hours, preferably 10–20 hours. This drying can be carried out under normal pressure or under reduced pressure.

[0030] Furthermore, the nanosheet MOR molecular sieve obtained after crystallization can be further processed by calcination to obtain sodium-type nanosheet MOR molecular sieve. The calcination can be carried out in any manner conventionally known in the art, for example, the calcination temperature is generally 300–800°C, preferably 400–650°C, and the calcination time is generally 1–10 hours, preferably 3–6 hours. In addition, the calcination is generally carried out in an oxygen-containing atmosphere, such as air or an oxygen atmosphere.

[0031] Furthermore, sodium-type nanosheet MOR molecular sieves are subjected to ammonium exchange via an ammonium salt solution, followed by calcination to prepare hydrogen-type MOR molecular sieves. The ammonium salt is selected from at least one of ammonium chloride, ammonium nitrate, ammonium carbonate, and ammonium sulfate; the ammonium ion concentration in the ammonium salt solution is 0.1–1 mol / L, and the solid-liquid ratio of sodium-type MOR to the ammonium salt solution is 1:5–1:20. After ion exchange at 30–80°C for 1–8 hours, the solid is separated, and the exchange is repeated 0–2 times to obtain ammonium-type MOR molecular sieves. The ammonium-type MOR molecular sieves are then calcined to obtain hydrogen-type MOR molecular sieves.

[0032] A third aspect of the present invention also provides a molecular sieve composition comprising a MOR molecular sieve prepared according to any of the methods described in the first aspect or according to any of the methods described in the second aspect, and a binder.

[0033] The fourth aspect of the present invention also provides the use of MOR molecular sieves prepared according to any of the methods described in the first aspect above, or MOR molecular sieves prepared according to any of the methods described in the second aspect above, or molecular sieve compositions described in the third aspect above, as adsorbents or catalysts for the conversion of organic compounds.

[0034] Compared with the prior art, the present invention has the following advantages:

[0035] The aluminum content at the T3 site of the eight-membered ring in the framework of the nanosheet MOR molecular sieve of this invention is higher than 65% of the total aluminum content. Furthermore, the nanosheet MOR molecular sieve of this invention has a nanosheet morphology, with an average crystal particle size not exceeding 600 nm and an average nanosheet thickness not exceeding 30 nm, exhibiting a unique crystal morphology.

[0036] The preparation method of this invention provides a simple and feasible method for preparing nanosheet MOR molecular sieves. This method can be directly synthesized using inexpensive and simple organic structure directing agent dimethyl diethylammonium ions. In addition, through the reasonable ratio of each raw material and the synergistic effect of aluminum sources with specific properties, the synthesized nanosheet MOR molecular sieves have a high yield, more framework aluminum on the eight-membered ring, high acidity, and more strong acids. Attached Figure Description

[0037] Figure 1The X-ray diffraction (XRD) pattern of the sample in Example 1;

[0038] Figure 2 The sample in Example 1 27 Al solid NMR spectrum ( 27 Al NMR);

[0039] Figure 3 The image shown is a scanning electron microscope (SEM) image of the sample in Example 1.

[0040] Figure 4 The X-ray diffraction (XRD) pattern of the sample in Example 2;

[0041] Figure 5 The image shown is a scanning electron microscope (SEM) image of the sample in Example 2.

[0042] Figure 6 The X-ray diffraction (XRD) pattern of the sample in Example 3;

[0043] Figure 7 The image shown is a scanning electron microscope (SEM) image of the sample in Example 3.

[0044] Figure 8 The X-ray diffraction (XRD) pattern of the sample in Example 4;

[0045] Figure 9 The image shown is a scanning electron microscope (SEM) image of the sample in Example 4.

[0046] Figure 10 The image shows a scanning electron microscope (SEM) image of the sample in Comparative Example 1.

[0047] Figure 11 The X-ray diffraction (XRD) pattern of the sample in Comparative Example 2 is shown.

[0048] Figure 12 The image shows a scanning electron microscope (SEM) image of the sample in Comparative Example 3.

[0049] Figure 13 This is a scanning electron microscope (SEM) image of the sample in Comparative Example 4. Detailed Implementation

[0050] According to the present invention, the aforementioned molecular sieve can be used in any physical form, such as powder, granules, or molded forms (e.g., strips, cloverleaf shapes, etc.). These physical forms can be obtained in any manner conventionally known in the art, without particular limitation. In the context of this specification, the structure of the nanosheet MOR molecular sieve is determined by X-ray diffraction (XRD), which is measured using an X-ray powder diffractometer. Before sample testing, the crystallization of the molecular sieve sample is observed using a scanning electron microscope (SEM) to confirm that the sample contains only one type of crystal, i.e., the molecular sieve sample is a pure phase. Based on this, XRD testing is then performed to ensure that there are no interfering peaks from other crystals in the diffraction peaks of the XRD pattern.

[0051] In the context of this specification, including in the following examples and comparative examples, the X-ray powder diffractometer used for the molecular sieves is a Panalytical X-PERPRO type X-ray powder diffractometer, used to analyze the phase composition of the samples, and a CuKα ray source. Nickel filter, 2θ scanning range 2~50°, operating voltage 40KV, current 40mA, scanning rate 10° / min.

[0052] In the context of this specification, including in the following examples and comparative examples, the scanning electron microscope (SEM) used for the molecular sieves is an S-4800II field emission scanning electron microscope. The molecular sieves were observed using this SEM at a magnification of 40,000x. A randomly selected field of view was used, and the average sum of the crystal diameters of all crystals within that field of view was calculated. This operation was repeated 10 times. The average sum of the 10 measurements was used as the crystal diameter. The thickness of all crystals within the same field of view was measured using the same method, and the percentage of crystals with a thickness not exceeding 25 nm was counted. This operation was repeated 5 times. The average of the 5 measurements was used as the percentage of crystals with a thickness not exceeding 25 nm.

[0053] In the context of this specification, including in the following examples and comparative examples, the micropore size, pore volume, specific surface area, and external specific surface area of ​​the molecular sieve were measured by the nitrogen physical adsorption-desorption method (BET method): the nitrogen physical adsorption-desorption isotherm of the molecular sieve was measured using a Micromeretic ASAP2020M physical adsorption instrument, and then calculated using the BET equation and t-plot equation. The experimental conditions for this molecular sieve were: measurement temperature -196℃, and before measurement, the molecular sieve was heat-treated at 550℃ in air for 6 hours, followed by pretreatment in vacuum at 350℃ for 4 hours.

[0054] In the context of this specification, including in the following examples and comparative examples, the molecular sieve was analyzed using an inductively coupled plasma atomic emission spectrometer (ICP) model Varian 725-ES, and the elemental content, in molar terms, was determined by dissolving the analytical sample in hydrofluoric acid.

[0055] In the context of this specification, including the following examples and comparative examples, the acid content of the molecular sieves was determined using an Altamira AMI-3300 instrument with NH3-TPD chemisorption-desorption curves. Before testing, the samples were activated at 550°C for 1 hour, ammonia was adsorbed at 100°C for 20 minutes, and then desorbed and detected at 100–600°C. By analyzing the Gaussian peak distribution, the acid content corresponding to desorption temperatures above 300°C was considered the acid content of strong acids.

[0056] In the context of this specification, including in the following examples and comparative examples, the yield of molecular sieves refers to the percentage of the mass of the calcined sample relative to the sum of the masses of SiO2 and Al2O3 contained in the raw material.

[0057] In the context of this specification, including in the following examples and comparative examples, the content of framework aluminum and non-framework aluminum in the molecular sieve is determined by... 27 Measured using an Al NMR spectrometer (Bruker Avance Ⅲ / WB-400), peaks with chemical shifts around 0 ppm corresponded to non-framework aluminum, while peaks with chemical shifts in the range of 65–35 ppm corresponded to framework aluminum. The percentage of the non-framework aluminum peak area relative to the sum of the two peak areas (total peak area) represents the non-framework aluminum content. Simultaneously, by Gaussian peak division, the percentage of the area corresponding to the peak with a chemical shift around 53.5 ppm relative to the total peak area represents the aluminum content at the T3 site of the eight-membered ring in the framework. The following examples further illustrate the invention in detail, but the invention is not limited to these examples.

[0058] Example 1

[0059] A mixture was prepared by stirring 16.85 g of deionized water, 0.855 g of sodium aluminate (containing 40.5 wt% Al₂O₃ and 30.6 wt% Na₂O), 0.497 g of sodium hydroxide, 4.05 g of dimethyl diethyl ammonium hydroxide solution (containing 25.0 wt% dimethyl diethyl ammonium hydroxide) (organic structure directing agent R), and 12.75 g of silica sol (containing 40.0 wt% SiO₂) at room temperature for 3 hours. The final material ratio (molar ratio) was as follows:

[0060] SiO2 / Al2O3 = 25;

[0061] NaOH / SiO2 = 0.24;

[0062] R (dimethyldiethylammonium ion meter) / SiO2 = 0.10;

[0063] H2O / SiO2 = 18.

[0064] The mixture was placed in a stainless steel reactor and heated at 170°C and 20 rpm for 3 days to crystallize. After crystallization, the mixture was filtered, washed, dried overnight in an oven at 100°C, and then calcined in air at 550°C for 6 hours. The XRD pattern of the product is shown below. Figure 1 The image shows a molecular sieve with a MOR structure. The yield of the MOR molecular sieve was 86 wt%. The SiO2 / Al2O3 molar ratio of the molecular sieve was determined to be 24.8 using inductively coupled plasma atomic emission spectrometry (ICP). The sample... 27 Al NMR spectrum as shown Figure 2 As shown, the aluminum content located at the T3 site of the eight-membered ring in the MOR molecular sieve framework accounts for 76% of the total aluminum content. The SEM image of the sample is shown below. Figure 3 As shown, the crystals exhibit a nanosheet morphology with an average crystal size of 260 nm and an average nanosheet thickness of 20 nm, resulting in an aspect ratio of 13. Furthermore, sheet-like crystals with a thickness not exceeding 25 nm account for 70% of the total number of crystals. The molecular sieve has a specific surface area of ​​488 m². 2 / gram, with an external specific surface area of ​​52 m² measured by the BET method. 2 / g; Total pore volume 0.42cm 3 / gram, micropore volume is 0.18 cm³ 3 / g. Sodium-type nanosheet MOR molecular sieves were subjected to ammonium ion exchange with 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 65℃ for 2 hours, followed by centrifugation and washing. The ammonium ion exchange was repeated twice. The resulting sample was dried overnight at 100℃ and calcined in air at 550℃ for 4 hours to obtain hydrogen-type nanosheet MOR molecular sieve samples. NH3-TPD analysis showed that the total acid content of the molecular sieve was 1127 μmol / g, and the strong acid content was 645 μmol / g.

[0065] Example 2

[0066] A mixture was prepared by stirring 9.45 g of deionized water, 0.694 g of sodium aluminate (containing 40.5 wt% Al₂O₃ and 30.6 wt% Na₂O), 0.569 g of sodium hydroxide, 3.94 g of dimethyl diethyl ammonium hydroxide solution (containing 25.00 wt% dimethyl diethyl ammonium hydroxide) (organic structure directing agent R), and 10.35 g of silica sol (containing 40.0 wt% SiO₂) at room temperature for 3 hours. The final material ratio (molar ratio) was as follows:

[0067] SiO2 / Al2O3 = 25;

[0068] NaOH / SiO2 = 0.30;

[0069] R(dimethyldiethylammonium ion) / SiO2 = 0.12;

[0070] H2O / SiO2 = 15.

[0071] The mixture was placed in a stainless steel reactor and heated at 165°C and 10 rpm for 5 days to crystallize. After crystallization, the mixture was filtered, washed, dried overnight in an oven at 100°C, and then calcined in air at 550°C for 6 hours. The XRD pattern of the product is shown below. Figure 4 The image shows a molecular sieve with a MOR structure. The yield of the MOR molecular sieve was 87 wt%. The SiO2 / Al2O3 molar ratio of the molecular sieve was determined to be 25.1 using inductively coupled plasma atomic emission spectrometry (ICP). The sample... 27 Al NMR spectrum and Figure 2 Similarly, in MOR molecular sieves, the aluminum content located at the T3 site of the eight-membered ring in the framework accounts for 72% of the total aluminum content. SEM images of the samples are shown below. Figure 5 As shown, the crystals exhibit a nanosheet morphology with an average crystal size of 240 nm and an average nanosheet thickness of 20 nm. The aspect ratio is 12, and sheet-like crystals with a thickness not exceeding 25 nm account for 65% of the total number of crystals. The specific surface area of ​​the molecular sieve is 506 m². 2 / gram, with an external specific surface area of ​​56 m² measured by the BET method. 2 / g; Total pore volume 0.44cm 3 / gram, micropore volume is 0.18 cm³ 3 / g. Sodium-type nanosheet MOR molecular sieves were subjected to ammonium ion exchange with 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 65℃ for 2 hours, followed by centrifugation and washing. The ammonium ion exchange was repeated twice. The resulting sample was dried overnight at 100℃ and calcined in air at 550℃ for 4 hours to obtain hydrogen-type nanosheet MOR molecular sieve samples. NH3-TPD analysis showed that the total acid content of the molecular sieve was 1154 μmol / g, and the strong acid content was 632 μmol / g.

[0072] Example 3

[0073] 21.80 g of deionized water, 0.857 g of sodium aluminate (containing 40.5 wt% Al₂O₃ and 30.6 wt% Na₂O), 0.907 g of sodium hydroxide, 3.65 g of dimethyl diethyl ammonium hydroxide solution (containing 25.00 wt% dimethyl diethyl ammonium hydroxide) (organic structure directing agent R), and 12.79 g of silica sol (containing 40.0 wt% SiO₂) were stirred at room temperature for 3 hours to obtain a mixture. The final material ratio (molar ratio) was:

[0074] SiO2 / Al2O3 = 25;

[0075] NaOH / SiO2 = 0.36;

[0076] R (dimethyldiethylammonium ion meter) / SiO2 = 0.09;

[0077] H2O / SiO2 = 21.

[0078] The mixture was placed in a stainless steel reactor and heated at 175°C and 30 rpm for 1.5 days to crystallize. After crystallization, the mixture was filtered, washed, dried overnight in an oven at 100°C, and then calcined in air at 550°C for 6 hours. The XRD pattern of the product is shown below. Figure 6 The image shows a molecular sieve with a MOR structure. The yield of the molecular sieve was 85 wt%. The SiO2 / Al2O3 molar ratio of the molecular sieve was determined to be 25.3 using inductively coupled plasma atomic emission spectrometry (ICP). The sample... 27 Al NMR spectrum and Figure 2 Similarly, in MOR molecular sieves, the aluminum content located at the T3 site of the eight-membered ring in the framework accounts for 71% of the total aluminum content. SEM images of the samples are shown below. Figure 7 As shown, the crystals exhibit a nanosheet morphology with an average crystal size of 330 nm and an average nanosheet thickness of 20 nm, resulting in an aspect ratio of 17. Furthermore, sheet-like crystals with a thickness not exceeding 25 nm account for 75% of the total number of crystals. The molecular sieve has a specific surface area of ​​479 m². 2 / gram, with an external specific surface area of ​​61 m² measured by the BET method. 2 / g; Total pore volume 0.46cm 3 / gram, micropore volume is 0.17 cm³ 3 / g. Sodium-type nanosheet MOR molecular sieves were subjected to ammonium ion exchange with 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 65℃ for 2 hours, followed by centrifugation and washing. The ammonium ion exchange was repeated twice. The resulting sample was dried overnight at 100℃ and calcined in air at 550℃ for 4 hours to obtain hydrogen-type nanosheet MOR molecular sieve samples. NH3-TPD analysis showed that the total acid content of the molecular sieve was 1148 μmol / g, and the strong acid content was 638 μmol / g.

[0079] Example 4

[0080] 34.75 g of deionized water, 1.203 g of sodium aluminate (containing 40.5 wt% Al₂O₃ and 30.6 wt% Na₂O), 0.792 g of sodium hydroxide, 6.02 g of dimethyl diethyl ammonium hydroxide solution (containing 25.00 wt% dimethyl diethyl ammonium hydroxide) (organic structure directing agent R), and 17.23 g of silica sol (containing 40.0 wt% SiO₂) were stirred at room temperature for 3 hours to obtain a mixture. The final material ratio (molar ratio) was:

[0081] SiO2 / Al2O3 = 24;

[0082] NaOH / SiO2 = 0.27;

[0083] R(dimethyldiethylammonium ion) / SiO2 = 0.11;

[0084] H2O / SiO2 = 24.

[0085] The mixture was placed in a stainless steel reactor and heated at 170°C and 40 rpm for 2.5 days to crystallize. After crystallization, the mixture was filtered, washed, dried overnight in an oven at 100°C, and then calcined in air at 550°C for 6 hours. The XRD pattern of the product is shown below. Figure 8 The image shows a molecular sieve with a MOR structure. The yield of the molecular sieve was 90 wt%. The SiO2 / Al2O3 molar ratio of the molecular sieve was determined to be 24.2 using inductively coupled plasma atomic emission spectrometry (ICP). The sample... 27 Al NMR spectrum and Figure 2 Similarly, in MOR molecular sieves, the aluminum content located at the T3 site of the eight-membered ring in the framework accounts for 74% of the total aluminum content. SEM images of the samples are shown below. Figure 9 As shown, the crystals exhibit a nanosheet morphology with an average crystal size of 180 nm and an average nanosheet thickness of 18 nm. The aspect ratio is 10, and sheet-like crystals with a thickness not exceeding 20 nm account for 60% of the total number of crystals. The specific surface area of ​​the molecular sieve is 473 m². 2 / gram, with an external specific surface area of ​​53 m² measured by the BET method. 2 / g; Total pore volume 0.52cm 3 / gram, micropore volume is 0.19 cm³ 3 / g. Sodium-type nanosheet MOR molecular sieves were subjected to ammonium ion exchange with 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 65℃ for 2 hours, followed by centrifugation and washing. The ammonium ion exchange was repeated twice. The resulting sample was dried overnight at 100℃ and calcined in air at 550℃ for 4 hours to obtain hydrogen-type nanosheet MOR molecular sieve samples. NH3-TPD analysis showed that the total acid content of the molecular sieve was 1164 μmol / g, and the strong acid content was 651 μmol / g.

[0086] Example 5

[0087] A mixture was prepared by stirring 44.61 g of deionized water, 1.241 g of sodium aluminate (containing 40.5 wt% Al₂O₃ and 30.6 wt% Na₂O), 0.737 g of sodium hydroxide, 10.23 g of dimethyldiethylammonium bromide solution (containing 25.00 wt% dimethyldiethylammonium bromide) (organic structure directing agent R), and 14.06 g of silica sol (containing 40.0 wt% SiO₂) at room temperature for 3 hours. The final material ratio (molar ratio) was as follows:

[0088] SiO2 / Al2O3 = 19;

[0089] NaOH / SiO2 = 0.32;

[0090] R(dimethyldiethylammonium ion) / SiO2 = 0.15;

[0091] H2O / SiO2 = 36.

[0092] The mixture was placed in a stainless steel reactor and heated to 175°C at 15 rpm for one day for crystallization. After crystallization, it was filtered, washed, dried overnight in an oven at 100°C, and then calcined in air at 550°C for 6 hours. The XRD pattern of the product obtained was similar to... Figure 1 Similarly, the molecular sieve exhibits a MOR structure. The yield of the molecular sieve was 87 wt%. The SiO2 / Al2O3 molar ratio of the molecular sieve was determined to be 19.4 using inductively coupled plasma atomic emission spectrometry (ICP). The sample... 27 Al NMR spectrum and Figure 2 Similarly, in MOR molecular sieves, the aluminum content located at the T3 site of the eight-membered ring in the framework accounts for 71% of the total aluminum content. The SEM image of the sample is similar to... Figure 3 Similarly, the crystals exhibit a nanosheet morphology, with an average crystal size of 350 nm and an average nanosheet thickness of 20 nm. The aspect ratio is 18, and sheet-like crystals with a thickness not exceeding 25 nm account for 70% of the total number of crystals. The specific surface area of ​​the molecular sieve is 492 m². 2 / gram, with an external specific surface area of ​​48 m² measured by the BET method. 2 / g; Total pore volume 0.50cm 3 / gram, micropore volume is 0.17 cm³ 3 / g. Sodium-type nanosheet MOR molecular sieve was subjected to ammonium ion exchange with 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 65℃ for 2 hours, followed by centrifugation and washing. The ammonium ion exchange was repeated twice. The resulting sample was dried overnight at 100℃ and calcined in air at 550℃ for 4 hours to obtain hydrogen-type nanosheet MOR molecular sieve sample. NH3-TPD analysis showed that the total acid content of the molecular sieve was 1362 μmol / g, and the strong acid content was 689 μmol / g.

[0093] Example 6

[0094] A mixture was prepared by stirring 45.33 g of deionized water, 1.161 g of sodium aluminate (containing 40.5 wt% Al₂O₃ and 30.6 wt% Na₂O), 0.705 g of sodium hydroxide, 7.82 g of dimethyl diethyl ammonium chloride solution (containing 25.00 wt% dimethyl diethyl ammonium chloride) (organic structure directing agent R), and 15.24 g of silica sol (containing 40.0 wt% SiO₂) at room temperature for 3 hours. The final material ratio (molar ratio) was:

[0095] SiO2 / Al2O3 = 22;

[0096] NaOH / SiO2 = 0.28;

[0097] R(dimethyldiethylammonium ion) / SiO2 = 0.14;

[0098] H2O / SiO2 = 33.

[0099] The mixture was placed in a stainless steel reactor and heated at 165°C and 50 rpm for 3.56 days to crystallize. After crystallization, the mixture was filtered, washed, dried overnight in an oven at 100°C, and then calcined in air at 550°C for 6 hours. The XRD pattern of the product obtained was similar to... Figure 1 Similarly, this is a molecular sieve with a MOR structure. The yield of the molecular sieve was 85 wt%. The SiO2 / Al2O3 molar ratio of the molecular sieve was determined to be 21.7 using inductively coupled plasma atomic emission spectrometry (ICP). The sample... 27 Al NMR spectrum and Figure 2 Similarly, in MOR molecular sieves, the aluminum content located at the T3 site of the eight-membered ring in the framework accounts for 70% of the total aluminum content. The SEM image of the sample is similar to... Figure 3 Similarly, the crystals exhibit a nanosheet morphology, with an average crystal size of 280 nm and an average nanosheet thickness of 18 nm. The aspect ratio is 16, and sheet-like crystals with a thickness not exceeding 20 nm account for 60% of the total number of crystals. The molecular sieve has a specific surface area of ​​475 m². 2 / gram, with an external specific surface area of ​​43 m² measured by the BET method. 2 / g; Total pore volume 0.49 cm 3 / gram, micropore volume is 0.18 cm³ 3 / g. Sodium-type nanosheet MOR molecular sieve was subjected to ammonium ion exchange with 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 65℃ for 2 hours, followed by centrifugation and washing. The ammonium ion exchange was repeated twice. The resulting sample was dried overnight at 100℃ and calcined in air at 550℃ for 4 hours to obtain hydrogen-type nanosheet MOR molecular sieve sample. NH3-TPD analysis showed that the total acid content of the molecular sieve was 1235 μmol / g, and the strong acid content was 667 μmol / g.

[0100] Example 7

[0101] 22.05 g of deionized water, 0.929 g of sodium aluminate (containing 40.5 wt% Al₂O₃ and 30.6 wt% Na₂O), 0.806 g of sodium hydroxide, 10.49 g of dimethyldiethylammonium bromide solution (containing 25.00 wt% dimethyldiethylammonium bromide) (organic structure directing agent R), and 16.63 g of silica sol (containing 40.0 wt% SiO₂) were stirred at room temperature for 3 hours to obtain a mixture. The final material ratio (molar ratio) was:

[0102] SiO2 / Al2O3 = 30;

[0103] NaOH / SiO2 = 0.26;

[0104] R(dimethyldiethylammonium ion) / SiO2 = 0.13;

[0105] H2O / SiO2 = 20.

[0106] The mixture was placed in a stainless steel reactor and heated at 160°C and 30 rpm for 6.5 days to crystallize. After crystallization, it was filtered, washed, dried overnight in an oven at 100°C, and then calcined in air at 550°C for 6 hours. The XRD pattern of the product obtained was similar to... Figure 1 Similarly, the molecular sieve exhibits a MOR structure. The yield of the molecular sieve was 84 wt%. Inductively coupled plasma atomic emission spectrometry (ICP) determined the SiO2 / Al2O3 molar ratio of the molecular sieve to be 30.1. The sample... 27 Al NMR spectrum and Figure 2 Similarly, in MOR molecular sieves, the aluminum content located at the T3 site of the eight-membered ring in the framework accounts for 74% of the total aluminum content. The SEM image of the sample is similar to... Figure 3 Similarly, the crystals exhibit a nanosheet morphology, with an average crystal size of 220 nm and an average nanosheet thickness of 18 nm. The aspect ratio is 12, and sheet-like crystals with a thickness not exceeding 25 nm account for 75% of the total number of crystals. The molecular sieve has a specific surface area of ​​465 m². 2 / gram, with an external specific surface area of ​​59 m² measured by the BET method.2 / g; Total pore volume 0.57cm 3 / gram, micropore volume is 0.17 cm³ 3 / g. Sodium-type nanosheet MOR molecular sieves were subjected to ammonium ion exchange with 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 65℃ for 2 hours, followed by centrifugation and washing. The ammonium ion exchange was repeated twice. The resulting sample was dried overnight at 100℃ and calcined in air at 550℃ for 4 hours to obtain hydrogen-type nanosheet MOR molecular sieve samples. NH3-TPD analysis showed that the total acid content of the molecular sieve was 1041 μmol / g, and the strong acid content was 549 μmol / g.

[0107] Example 8

[0108] 38.19 g of deionized water, 0.800 g of sodium aluminate (containing 40.5 wt% Al₂O₃ and 30.6 wt% Na₂O), 0.751 g of sodium hydroxide, 4.50 g of dimethyl diethyl ammonium chloride solution (containing 25.00 wt% dimethyl diethyl ammonium chloride) (organic structure directing agent R), and 15.75 g of silica sol (containing 40.0 wt% SiO₂) were stirred at room temperature for 3 hours to obtain a mixture. The final material ratio (molar ratio) was:

[0109] SiO2 / Al2O3 = 33;

[0110] NaOH / SiO2 = 0.25;

[0111] R (dimethyldiethylammonium ion meter) / SiO2 = 0.09;

[0112] H2O / SiO2 = 27.

[0113] The mixture was placed in a stainless steel reactor and heated at 165°C and 10 rpm for 5 days to crystallize. After crystallization, it was filtered, washed, dried overnight in an oven at 100°C, and then calcined in air at 550°C for 6 hours. The XRD pattern of the product obtained was similar to... Figure 1 Similarly, this is a molecular sieve with a MOR structure. The yield of the molecular sieve was 86 wt%. The SiO2 / Al2O3 molar ratio of the molecular sieve was determined to be 32.5 using inductively coupled plasma atomic emission spectrometry (ICP). The sample... 27 Al NMR spectrum and Figure 2 Similarly, in MOR molecular sieves, the aluminum content located at the T3 site of the eight-membered ring in the framework accounts for 75% of the total aluminum content. The SEM image of the sample is similar to... Figure 3 Similarly, the crystals exhibit a nanosheet morphology, with an average crystal size of 410 nm and an average nanosheet thickness of 20 nm. The aspect ratio is 21, and sheet-like crystals with a thickness not exceeding 25 nm account for 65% of the total number of crystals. The molecular sieve has a specific surface area of ​​513 m².2 / gram, with an external specific surface area of ​​45 m² measured by the BET method. 2 / g; Total pore volume 0.55cm 3 / gram, micropore volume is 0.19 cm³ 3 / g. Sodium-type nanosheet MOR molecular sieve was subjected to ammonium ion exchange with 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 65℃ for 2 hours, followed by centrifugation and washing. The ammonium ion exchange was repeated twice. The resulting sample was dried overnight at 100℃ and calcined in air at 550℃ for 4 hours to obtain hydrogen-type nanosheet MOR molecular sieve sample. NH3-TPD analysis showed that the total acid content of the molecular sieve was 949 μmol / g, and the strong acid content was 484 μmol / g.

[0114] Example 9

[0115] A mixture was prepared by stirring 41.59 g of deionized water, 0.923 g of sodium aluminate (containing 40.5 wt% Al₂O₃ and 30.6 wt% Na₂O), 1.053 g of sodium hydroxide, 6.22 g of dimethyl diethyl ammonium chloride solution (containing 25.00 wt% dimethyl diethyl ammonium chloride) (organic structure directing agent R), and 15.43 g of silica sol (containing 40.0 wt% SiO₂) at room temperature for 3 hours. The final material ratio (molar ratio) was as follows:

[0116] SiO2 / Al2O3 = 28;

[0117] NaOH / SiO2 = 0.34;

[0118] R(dimethyldiethylammonium ion) / SiO2 = 0.11;

[0119] H2O / SiO2 = 30.

[0120] The mixture was placed in a stainless steel reactor and heated to crystallize at 170°C and 25 rpm for 2 days. After crystallization, it was filtered, washed, dried overnight in an oven at 100°C, and then calcined in air at 550°C for 6 hours. The XRD pattern of the product obtained was similar to... Figure 1 Similarly, the molecular sieve exhibits a MOR structure. The yield of the molecular sieve was 89 wt%. Inductively coupled plasma atomic emission spectrometry (ICP) determined the SiO2 / Al2O3 molar ratio of the molecular sieve to be 27.6. The sample... 27 Al NMR spectrum and Figure 2 Similarly, in MOR molecular sieves, the aluminum content located at the T3 site of the eight-membered ring in the framework accounts for 72% of the total aluminum content. The SEM image of the sample is similar to... Figure 3Similarly, the crystals exhibit a nanosheet morphology, with an average crystal size of 380 nm and an average nanosheet thickness of 20 nm, resulting in an aspect ratio of 19. Furthermore, sheet-like crystals with a thickness not exceeding 25 nm account for 80% of the total number of crystals counted. The molecular sieve has a specific surface area of ​​459 m². 2 / gram, with an external specific surface area of ​​47 m² measured by the BET method. 2 / g; Total pore volume 0.48cm 3 / gram, micropore volume is 0.18 cm³ 3 / g. Sodium-type nanosheet MOR molecular sieves were subjected to ammonium ion exchange with 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 65℃ for 2 hours, followed by centrifugation and washing. The ammonium ion exchange was repeated twice. The resulting sample was dried overnight at 100℃ and calcined in air at 550℃ for 4 hours to obtain hydrogen-type nanosheet MOR molecular sieve samples. NH3-TPD analysis showed that the total acid content of the molecular sieve was 990 μmol / g, and the strong acid content was 503 μmol / g.

[0121] Comparative Example 1

[0122] Compared to Example 1, everything else is the same, except that the final material ratio (molar ratio) is:

[0123] SiO2 / Al2O3 = 10;

[0124] NaOH / SiO2 = 0.24;

[0125] R / SiO2 = 0.10;

[0126] H2O / SiO2 = 18.

[0127] The mixture was placed in a stainless steel reactor and heated at 170°C and 20 rpm for 3 days to crystallize. After crystallization, the mixture was filtered, washed, and dried overnight in an oven at 100°C. The XRD pattern of the obtained product was compared with... Figure 1 Similarly, it is a MOR molecular sieve, but the SEM image of the sample is as follows. Figure 10 As shown, the molecular sieve has a rod-like morphology, not a nanosheet-like molecular sieve. The sample was subjected to... 27 AlNMR analysis showed that the aluminum content located at the T3 site of the eight-membered ring in the molecular sieve was 52% of the total aluminum content. (Comparative Example 2)

[0128] The material ratio is the same as in Example 5, except that less organic structure-directing agent R is added. The final material ratio (molar ratio) is:

[0129] SiO2 / Al2O3 = 19;

[0130] NaOH / SiO2 = 0.32;

[0131] R / SiO2 = 0.05;

[0132] H2O / SiO2 = 36.

[0133] The mixture was placed in a stainless steel reactor and heated to 175°C at 15 rpm for one day for crystallization. After crystallization, the mixture was filtered, washed, dried overnight in an oven at 100°C, and then calcined in air at 550°C for 6 hours. The XRD pattern of the product is shown below. Figure 11 As shown, the sample did not crystallize and had an amorphous structure, therefore it is not a MOR molecular sieve.

[0134] Comparative Example 3

[0135] The material ratio is the same as in Example 2, except that tetraethylammonium hydroxide is added as the organic structure directing agent R. The final material ratio (molar ratio) is:

[0136] SiO2 / Al2O3 = 25;

[0137] NaOH / SiO2 = 0.30;

[0138] R (tetraethylammonium ion) / SiO2 = 0.12;

[0139] H2O / SiO2 = 15.

[0140] The mixture was placed in a stainless steel reactor and heated at 165°C and 10 rpm for 5 days to crystallize. After crystallization, it was filtered, washed, and dried overnight in an oven at 100°C. The XRD pattern of the obtained product was compared with... Figure 1 Similarly, it is a MOR molecular sieve, but the SEM image of the sample is as follows. Figure 12 As shown, the molecular sieve has a rod-like morphology, not a nanosheet-like molecular sieve. The sample was subjected to... 27 AlNMR analysis showed that the aluminum content located at the T3 site of the eight-membered ring in the molecular sieve was 44% of the total aluminum content.

[0141] Comparative Example 4

[0142] The material ratio is the same as in Example 5, except that the content of Al2O3 and Na2O in the added sodium aluminate is different. The sodium aluminate composition is 50.6% by weight of Al2O3 and 45.2% by weight of Na2O. The raw materials are prepared in the same amount of substances, and the final material ratio (molar ratio) is:

[0143] SiO2 / Al2O3 = 19;

[0144] NaOH / SiO2 = 0.32;

[0145] R / SiO2 = 0.15;

[0146] H2O / SiO2 = 36.

[0147] The mixture was placed in a stainless steel reactor and heated at 175°C and 15 rpm for one day to crystallize. After crystallization, it was filtered, washed, and dried overnight in an oven at 100°C. The XRD pattern of the obtained product was compared with... Figure 1 Similarly, it is a MOR molecular sieve, but the SEM image of the sample is as follows. Figure 13 As shown, the molecular sieve has a granular morphology, not a nanosheet molecular sieve. The sample was subjected to... 27 AlNMR analysis showed that the aluminum content located at the T3 site of the eight-membered ring in the molecular sieve was 47% of the total aluminum content.

[0148] The specific embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combining the various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A MOR molecular sieve, characterized in that, The aluminum content located at the T3 site of the eight-membered ring in the molecular sieve is higher than 65% of the total aluminum mass content; The method for preparing the molecular sieve includes: A silicon source, an aluminum source, an alkali source, an organic structure directing agent R, and water are mixed and then crystallized to obtain a MOR molecular sieve. Wherein, the organic structure directing agent R is selected from at least one of dimethyl diethyl ammonium hydroxide, dimethyl diethyl ammonium chloride, dimethyl diethyl ammonium bromide or dimethyl diethyl ammonium iodide; The added silicon source is calculated as SiO2, the aluminum source as Al2O3, and the alkali source as OH. - The organic structure-directing agent R, calculated as dimethyldiethylammonium ions and water, is present in a molar ratio of SiO2:Al2O3:OH. - : R: H2O=1: 0.028~0.056: 0.15~0.38: 0.07~0.17: 10~50; The silicon source is silica sol; the aluminum source is sodium aluminate; the alkali source is sodium hydroxide or potassium hydroxide; The sodium aluminate contains 35% to 43% Al2O3 by weight and 25% to 33% Na2O by weight.

2. The molecular sieve according to claim 1, characterized in that, The aluminum content in the molecular sieve located at the T3 site of the eight-membered ring in the framework is 70% to 80% of the total aluminum mass content.

3. The molecular sieve according to claim 1, characterized in that, The molecular sieve has a nanosheet morphology, with an average crystal particle size of no more than 600 nm and an average nanosheet thickness of no more than 30 nm.

4. The molecular sieve according to claim 3, characterized in that, The molecular sieve has an average crystal size of 150~550nm and an average nanosheet thickness of 15~25nm.

5. The molecular sieve according to claim 3, characterized in that, In the molecular sieve, plate-like crystals with a thickness of no more than 25 nm account for at least 60% of the total number of crystals.

6. The molecular sieve according to claim 5, characterized in that, In the molecular sieve, plate-like crystals with a thickness of no more than 25 nm account for 60% to 90% of the total number of crystals.

7. The molecular sieve according to claim 3, characterized in that, The aspect ratio of the molecular sieve crystal is 8 to 35.

8. The molecular sieve according to claim 7, characterized in that, The aspect ratio of the molecular sieve crystal is 8 to 20.

9. The molecular sieve according to claim 1, characterized in that, The total specific surface area of ​​the molecular sieve is not less than 400 m². 2 / gram; and / or, The specific surface area of ​​the molecular sieve is not less than 30 m². 2 / gram; and / or, The total pore volume of the molecular sieve is not less than 0.30 cm³. 3 / gram; and / or, The molecular sieve has a micropore volume of not less than 0.15 cm³. 3 / gram.

10. The molecular sieve according to claim 9, characterized in that, The total specific surface area of ​​the molecular sieve is 400-600 m². 2 / gram; and / or, The molecular sieve has an external specific surface area of ​​30-100 m². 2 / gram; and / or, The total pore volume of the molecular sieve is 0.30~0.70 cm³. 3 / gram; and / or, The molecular sieve has a micropore volume of 0.15~0.25 cm³. 3 / gram.

11. The molecular sieve according to claim 1, characterized in that, The total acid content of the molecular sieve is not less than 800 μmol / g; and / or, The molecular sieve has a strong acid content of not less than 300 μmol / g.

12. The molecular sieve according to claim 11, characterized in that, The total acidity of the molecular sieve is 800~1500 μmol / g; and / or, The molecular sieve has a strong acid content of 300~700 μmol / g.

13. A method for preparing MOR molecular sieves, characterized in that, include: A silicon source, an aluminum source, an alkali source, an organic structure directing agent R, and water are mixed and then crystallized to obtain a MOR molecular sieve. Wherein, the organic structure directing agent R is selected from at least one of dimethyl diethyl ammonium hydroxide, dimethyl diethyl ammonium chloride, dimethyl diethyl ammonium bromide or dimethyl diethyl ammonium iodide; The added silicon source is calculated as SiO2, the aluminum source as Al2O3, and the alkali source as OH. - The organic structure-directing agent R, calculated as dimethyldiethylammonium ions and water, is present in a molar ratio of SiO2:Al2O3:OH. - : R: H2O=1: 0.028~0.056: 0.15~0.38: 0.07~0.17: 10~50; The silicon source is silica sol; the aluminum source is sodium aluminate; the alkali source is sodium hydroxide or potassium hydroxide; The sodium aluminate contains 35% to 43% Al2O3 by weight and 25% to 33% Na2O by weight.

14. The method according to claim 13, characterized in that, The organic structure directing agent R is dimethyldiethylammonium hydroxide.

15. The method according to claim 13, characterized in that, The sodium aluminate contains 38% to 43% Al2O3 by weight and 28% to 33% Na2O by weight.

16. The method according to claim 13, characterized in that, The crystallization treatment conditions include: crystallization at 150~190℃ for 0.75~8.0 days.

17. The method according to claim 16, characterized in that, The crystallization treatment conditions include: crystallization at 160~180℃ for 1.0~7.0 days.

18. A molecular sieve composition comprising the MOR molecular sieve according to any one of claims 1-12 or the MOR molecular sieve prepared by any one of claims 13-17, and a binder.

19. The MOR molecular sieve according to any one of claims 1-12, or the MOR molecular sieve prepared by any one of claims 13-17, or the molecular sieve composition according to claim 18, as an adsorbent or a catalyst for the conversion of organic compounds.

Citation Information

Patent Citations

  • Process for synthesis of nano mordenite molecular sieve

    CN100453461C

  • Synthesis of mercerized zeolite with high silicon content

    CN1020039C

  • Preparation method of layered nano-mordenite molecular sieve

    CN102718231B

  • A kind of method of synthesizing nanometer molecular sieve

    CN106698453B

  • Nano-aggregate lamellar zeolite

    CN107758685B