An ultrathin magnesium-iron super-stable mineralizer, a preparation method thereof and application thereof in remediation of arsenic-contaminated farmland
By calcining magnesium carbonate under a reducing gas to prepare magnesium oxide, which then reacts with iron compounds to form an ultrathin, ultrastable magnesium-iron mineralizer, the problems of low selectivity and wastewater pollution during the synthesis process of existing adsorbents are solved, thus achieving efficient remediation of arsenic-contaminated soil.
Patent Information
- Application Number
- CN202410078985.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-19
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-01-19
AI Technical Summary
Existing adsorbents have low selectivity and small adsorption capacity when treating arsenic-contaminated soil, and their synthesis process generates high COD wastewater, leading to environmental pollution and high preparation costs.
Magnesium oxide is prepared by calcining magnesium carbonate under reducing gas conditions and then reacting it with iron compounds in water to form an ultra-thin, ultra-stable magnesium-iron mineralizer. This avoids the generation of saline wastewater, increases the specific surface area, and improves adsorption activity.
It achieves zero saline wastewater generation, enhances the selectivity and adsorption capacity of the adsorbent, effectively reduces the bioavailability and mobility of arsenic, and realizes in-situ mineralization remediation of arsenic pollutants.
Smart Images

Figure CN117963994B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of heavy metal pollution control technology, and in particular to an ultrathin magnesium-iron ultra-stable mineralizer, its preparation method, and its application in the remediation of arsenic-contaminated farmland. Background Technology
[0002] Currently, heavy metal pollution in arable land is a serious problem. The main heavy metals include cadmium, nickel, and arsenic, with arsenic pollution being particularly prominent. Arsenic exists as highly toxic inorganic arsenic compounds. Due to the poor biodegradability, high mobility, and high bioavailability of inorganic arsenic, inorganic arsenic pollutants in the soil not only cannot be naturally degraded over long periods but can also enter food crops through the root system. Given arsenic's high toxicity and strong carcinogenicity (ranked first on the list of priority hazardous substances published by the U.S. Toxic Substances and Disease Registry (2019)), arsenic-contaminated food poses a serious threat to public health.
[0003] Currently, adsorption is the primary method for treating arsenic pollution, with the adsorbent being the key. Existing adsorbents mainly include natural minerals such as attapulgite, magnetite, hematite, and activated carbon. However, these natural minerals have low selectivity and small adsorption capacity, and are easily affected by interference from other ions during use, leading to a rapid decline in adsorption efficiency. Furthermore, due to the limitations of the mineral structure itself, the adsorption of arsenic by these natural minerals relies mainly on weak electrostatic attraction, and the adsorbed arsenic is easily desorbed when external conditions change, causing re-pollution. Compared to natural minerals, researchers have developed porous organometallic framework materials, porous polymer materials, and organic / inorganic composite materials for the remediation of arsenic pollution. While these synthetic materials have shown better selectivity and adsorption capacity, their synthesis involves the use of large amounts of organic matter, resulting in high-COD wastewater. This not only increases the production cost in wastewater treatment but also poses serious environmental pollution problems. Summary of the Invention
[0004] In view of this, the purpose of this invention is to provide an ultrathin magnesium-iron superstable mineralizer, its preparation method, and its application in the remediation of arsenic-contaminated farmland. The preparation method provided by this invention is simple to synthesize, produces no saline wastewater, effectively reduces the material preparation cost, and has excellent selectivity and adsorption capacity.
[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution:
[0006] This invention provides a method for preparing an ultrathin magnesium-iron superstable mineralizer, comprising the following steps:
[0007] Magnesium carbonate is calcined under reducing gas conditions to obtain magnesium oxide;
[0008] The magnesium oxide and iron compounds were dispersed in deionized water, and the first and second reactions were carried out sequentially to obtain the ultrathin magnesium-iron ultrastable mineralizer.
[0009] The calcination temperature is 400–600°C;
[0010] The iron compounds include ferric acetate and / or ferric citrate.
[0011] Preferably, the reducing gas includes hydrogen or carbon monoxide.
[0012] Preferably, the roasting time is 3 to 6 hours.
[0013] Preferably, the molar ratio of iron in the iron compound to magnesium in magnesium oxide is 1:4 to 1:2.
[0014] Preferably, the dispersion of magnesium oxide and iron compound in deionized water comprises: dispersing magnesium oxide in deionized water to obtain a magnesium oxide dispersion; dispersing iron compound in deionized water to obtain an iron compound solution; mixing the magnesium oxide dispersion and the iron compound solution; wherein the concentration of the magnesium oxide dispersion is 0.1–1.2 mol / L; and the concentration of the iron compound solution is 0.025–0.6 mol / L.
[0015] Preferably, the temperature of the first reaction is 30–60°C, and the time is 1–3 hours.
[0016] Preferably, the temperature of the second reaction is 110–160°C, and the time is 2–6 hours.
[0017] Preferably, after the second reaction, the method further includes: separating the obtained second reaction solution into solid and liquid phases, and freeze-drying the obtained solid.
[0018] The present invention also provides an ultrathin magnesium-iron superstable mineralizer prepared by the preparation method described above, wherein the ultrathin magnesium-iron superstable mineralizer exhibits an extremely thin two-dimensional sheet structure.
[0019] This invention also provides the application of the ultra-thin magnesium-iron super-stable mineralizer described in the above technical solution in the remediation of arsenic-contaminated farmland.
[0020] This invention provides a method for preparing an ultrathin magnesium-iron superstable mineralizer, comprising the following steps: calcining magnesium carbonate under reducing gas conditions to obtain magnesium oxide; dispersing the magnesium oxide and an iron compound in deionized water, and sequentially performing a first reaction and a second reaction to obtain the ultrathin magnesium-iron superstable mineralizer; the calcination temperature is 400–600°C; the iron compound includes ferric acetate and / or ferric citrate.
[0021] Beneficial effects
[0022] (1) No salt wastewater is generated: The acetate or citrate ions in the iron compounds selected in this invention will form CO2 in the high-temperature hydrothermal reaction, instead of producing inorganic anions, so no salt wastewater is generated during the reaction.
[0023] (2) The magnesium oxide of this invention is obtained by calcining magnesium carbonate at 400-600°C under a reducing gas atmosphere. This calcination effectively reduces the particle size of the obtained magnesium oxide, increases its specific surface area, and thus enhances its reactivity. The main reason is that under the condition of introducing a reducing atmosphere, the carbon dioxide produced by the thermal decomposition of magnesium carbonate reacts in situ with H2 or CO on the material surface, significantly reducing the decomposition temperature of magnesium carbonate and avoiding the sintering phenomenon of conventional methods, resulting in high activity of the generated magnesium oxide. In the preparation process of the ultrathin magnesium-iron superstable mineralizer, magnesium oxide, as a solid alkali, has high alkalinity, thus providing a magnesium source while ensuring the alkaline environment required for the synthesis of the mineralizer. The acetate and citrate ions in the selected ferric acetate or ferric citrate both have the effect of promoting the dispersion of inorganic nanomaterials; thus, the final ultrathin magnesium-iron superstable mineralizer has a high specific surface area, can expose more active sites, and is beneficial for the adsorption of heavy metal arsenic. At the same time, since iron and magnesium elements are more likely to combine with arsenic, they can exhibit better selectivity and long-lasting effect.
[0024] (3) The preparation method provided by the present invention is simple to synthesize.
[0025] This invention also provides the application of the ultrathin magnesium-iron ultra-stable mineralizer described above in the remediation of arsenic-contaminated farmland. The ferric iron in the ultrathin magnesium-iron ultra-stable mineralizer of this invention has excellent oxidizing ability, capable of oxidizing As(III) to easily removable As(V); furthermore, both magnesium and iron can form stable inner-shell compounds with As(V), thereby reducing the bioavailability and mobility of arsenic, achieving in-situ mineralization remediation of arsenic pollutants. Attached Figure Description
[0026] Figure 1 Here is a SEM image of the magnesium oxide prepared in Example 1;
[0027] Figure 2 The XRD pattern of the ultrathin magnesium-iron superstable mineralizer prepared in Example 1;
[0028] Figure 3 TEM image of the ultrathin magnesium-iron ultrastable mineralizer prepared in Example 1;
[0029] Figure 4 The attached diagram shows the nitrogen adsorption-desorption process of the ultrathin magnesium-iron ultrastable mineralizer prepared in Example 2.
[0030] Figure 5TEM image of the magnesium-iron superstable mineralizer prepared in Comparative Example 1. Detailed Implementation
[0031] This invention provides a method for preparing an ultrathin magnesium-iron superstable mineralizer, comprising the following steps:
[0032] Magnesium carbonate is calcined under reducing gas conditions to obtain magnesium oxide;
[0033] The magnesium oxide and iron compounds were dispersed in deionized water, and the first and second reactions were carried out sequentially to obtain the ultrathin magnesium-iron ultrastable mineralizer.
[0034] The roasting temperature is 400–600°C;
[0035] The iron compounds include ferric acetate and / or ferric citrate.
[0036] Unless otherwise specified, all raw materials used in this invention are preferably commercially available products.
[0037] In this invention, magnesium carbonate is calcined under reducing gas conditions to obtain magnesium oxide.
[0038] In this invention, the reducing gas preferably includes hydrogen or carbon monoxide, more preferably hydrogen. In this invention, the calcination temperature is 400–600°C, preferably 450–550°C; the calcination time is preferably 3–6 hours, more preferably 4–5 hours. In this invention, the calcination is preferably carried out in a tube furnace. After calcination, this invention preferably further includes cooling the furnace to room temperature.
[0039] After obtaining magnesium oxide, the present invention disperses the magnesium oxide and iron compound in deionized water and performs the first reaction and the second reaction in sequence to obtain the ultrathin magnesium-iron ultrastable mineralizer.
[0040] In this invention, the iron compound comprises ferric acetate and / or ferric citrate, preferably ferric acetate. In this invention, the molar ratio of iron to magnesium in the iron compound is preferably 1:4 to 1:2.
[0041] In this invention, the dispersion of magnesium oxide and iron compound in deionized water preferably comprises: dispersing magnesium oxide in deionized water to obtain a magnesium oxide dispersion; dispersing the iron compound in deionized water to obtain an iron compound solution; and mixing the magnesium oxide dispersion and the iron compound solution. In this invention, the concentration of the magnesium oxide dispersion is preferably 0.1–1.2 mol / L; and the concentration of the iron compound solution is preferably 0.025–0.6 mol / L.
[0042] In this invention, the temperature of the first reaction is preferably 30-60°C, more preferably 40-50°C; the time is preferably 1-3 hours; and the first reaction is preferably carried out under stirring conditions.
[0043] In this invention, the first reaction process preferably involves the following reaction:
[0044] MgO + H₂O = Mg(OH)₂
[0045] Fe 3+ +Mg(OH)2+CO3 2- +OH-→MgFe(OH)3CO3
[0046] In this invention, the temperature of the second reaction is preferably 110–160°C, more preferably 120–150°C, and even more preferably 130–140°C; the time is preferably 2–6 hours. In this invention, the second reaction process mainly involves crystallization, which promotes faster growth of the magnesium-iron ultrastable mineralized material along the ab plane.
[0047] Following the second reaction, the present invention preferably further includes: solid-liquid separation of the obtained second reaction solution, and freeze-drying of the obtained solid. In the present invention, the solid-liquid separation is preferably filtration. In the present invention, the freeze-drying is preferably vacuum freeze-drying.
[0048] The present invention also provides an ultrathin magnesium-iron superstable mineralizer prepared by the preparation method described above, wherein the ultrathin magnesium-iron superstable mineralizer exhibits an extremely thin two-dimensional sheet structure.
[0049] This invention also provides the application of the ultra-thin magnesium-iron super-stable mineralizer described in the above technical solution in the remediation of arsenic-contaminated farmland.
[0050] In this invention, the application preferably includes the following steps:
[0051] The soil to be treated is mixed with an ultra-thin magnesium-iron ultra-stable mineralizer and then treated.
[0052] In this invention, the mass ratio of the soil to be treated to the ultra-thin magnesium-iron ultra-stable mineralizer is preferably 1000:1 to 100:1, and more preferably 500:1.
[0053] The following detailed description, in conjunction with embodiments, illustrates the ultra-thin magnesium-iron super-stable mineralizer provided by the present invention, its preparation method, and its application in the remediation of arsenic-contaminated farmland. However, these descriptions should not be construed as limiting the scope of protection of the present invention.
[0054] Example 1
[0055] A ceramic boat containing 16.8g of magnesium carbonate was placed in a tube furnace and calcined at 400℃ for 4 hours under H2 conditions to obtain magnesium oxide.
[0056] Weigh 0.8g of the above magnesium oxide and add it to 100mL of deionized water. Sonicate the mixture to obtain a uniform magnesium oxide suspension (molar concentration of 0.2mol / L).
[0057] Weigh 2.46 g of ferric acetate tetrahydrate and add it to 100 mL of deionized water. Sonicate the solution to obtain a clear ferric acetate solution (0.1 mol / L).
[0058] The magnesium oxide suspension and ferric acetate solution were rapidly poured into a stirred reactor and stirred at 50°C for 1 hour. The reactor was then heated to 160°C and held at that temperature for 6 hours, before being cooled to room temperature. The solid-liquid mixture was separated by centrifugation, and the precipitate was freeze-dried in a vacuum freeze dryer to obtain the ultra-thin, ultra-stable magnesium-iron mineralizer.
[0059] Figure 1 Here is a SEM image of magnesium oxide obtained under a reducing atmosphere, from... Figure 1 It can be seen that the obtained magnesium oxide is spherical with a particle size of 80-90 nm and is uniformly dispersed.
[0060] Figure 2 The XRD pattern of the prepared ultrathin magnesium-iron ultrastable mineralizer is shown below. Figure 2 It can be seen that the obtained material has a pure phase, and each diffraction peak is consistent with the standard pattern, with no obvious impurities, indicating the feasibility of the method.
[0061] Figure 3 TEM images of the prepared ultrathin magnesium-iron ultrastable mineralizer, by Figure 3 It can be seen that the prepared ultrathin magnesium-iron superstable mineralizer has a two-dimensional sheet structure and is distorted. In the TEM image, the ultrathin magnesium-iron superstable mineralizer is very close to the background color, indicating that the prepared magnesium-iron superstable mineralizer is very thin.
[0062] Example 2
[0063] Weigh 1.2g of magnesium oxide from Example 1 and add it to 100mL of deionized water. Sonicate the mixture to obtain a uniform magnesium oxide suspension (0.3mol / L molar concentration).
[0064] Weigh 3.35g of ferric citrate pentahydrate and add it to 100mL of deionized water. Sonicate the solution to obtain a clear ferric citrate solution (0.1mol / L).
[0065] The magnesium oxide suspension and ferric citrate solution were rapidly poured into a stirred reactor and stirred at 60°C for 3 hours. The reactor was then heated to 180°C and held at that temperature for 6 hours, before being cooled to room temperature. The solid-liquid mixture was separated by centrifugation, and the precipitate was freeze-dried in a vacuum freeze dryer to obtain the ultra-thin, ultra-stable magnesium-iron mineralizer.
[0066] Figure 4 The attached diagram shows the nitrogen adsorption-desorption process of the ultrathin magnesium-iron ultrastable mineralizer prepared in Example 2. Calculations show that its specific surface area is 162 m². 2 / g, the large specific surface area lays the foundation for increasing its mineralization.
[0067] Comparative Example 1
[0068] To further illustrate the superiority of magnesium oxide in the preparation method of this invention, a comparison was made between the magnesium-iron superstable mineralizer obtained in this invention and commercially available analytical grade magnesium oxide.
[0069] In this comparative example, all conditions are the same as those in Example 1, except for the source of magnesium oxide.
[0070] Figure 5 The TEM image shows the magnesium-iron ultrastable mineralizer prepared in Comparative Example 1. Figure 5 It can be seen that the material obtained using ordinary magnesium oxide is in the form of aggregated thick sheets. This further demonstrates the advantages of the method provided in this invention.
[0071] Application Example 1
[0072] Soil samples contaminated with arsenic were taken from the contaminated site. According to the national standard GB-15618-2008, the arsenic content in the soil exceeded the risk screening value by more than 10 times. 1000g of the pretreated soil sample was thoroughly mixed with 2g of the ultra-thin magnesium-iron ultra-stable mineralizer prepared in Example 1 in a 1L beaker, followed by the addition of 500mL of deionized water and natural placement. Samples were taken at regular intervals to measure the bioavailable content. After 7 days of remediation, the bioavailable content of As decreased from 0.278 mg / kg to 0.134 mg / kg, a reduction of 51.8%; after 14 days of remediation, the bioavailable content of As decreased to 0.106 mg / kg, a reduction of 61.9%; and after 28 days, the bioavailable content of As decreased to 0.083 mg / kg, a reduction of 70.1%.
[0073] Application Example 2
[0074] Soil samples contaminated with arsenic were taken from the contaminated site. According to the national standard GB-15618-2008, the arsenic content in the soil exceeded the risk screening value by more than 10 times. 1000g of the pretreated soil sample was thoroughly mixed with 2g of the ultra-thin magnesium-iron ultra-stable mineralizer prepared in Example 2 in a 1L beaker, and then 500mL of deionized water was added. The mixture was left to stand naturally, and samples were taken at regular intervals to measure its bioavailable content. After 7 days of remediation, the bioavailable content of As decreased from 0.278 mg / kg to 0.122 mg / kg, a decrease of 56.1%; after 14 days of remediation, the bioavailable content of As decreased to 0.099 mg / kg, a decrease of 64.4%; and after 28 days, the bioavailable content of As decreased to 0.076 mg / kg, a reduction of 72.7%.
[0075] Application Comparative Example 1
[0076] Soil samples contaminated with arsenic were taken from the contaminated site. According to the national standard GB-15618-2008, the arsenic content in the soil exceeded the risk screening value by more than 10 times. 1000g of the pretreated soil sample was thoroughly mixed with 2g of the magnesium-iron superstable mineralizer prepared in Comparative Example 1 in a 1L beaker, followed by the addition of 500mL of deionized water and natural placement. Samples were taken at regular intervals to measure the bioavailable arsenic content. After 7 days of remediation, the bioavailable arsenic content decreased from 0.278 mg / kg to 0.187 mg / kg, a decrease of 33.8%; after 14 days, it decreased to 0.169 mg / kg, a decrease of 39.2%; and after 28 days, it decreased to 0.157 mg / kg, a reduction of 43.5%.
[0077] The above data shows that the ultrathin magnesium-iron super-stable mineralizer can significantly reduce the available As content in the soil in a short period of time, demonstrating excellent remediation performance.
[0078] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing an ultrathin magnesium-iron superstable mineralizer, characterized in that, Includes the following steps: Magnesium carbonate is calcined under reducing gas conditions to obtain magnesium oxide; The magnesium oxide and iron compounds were dispersed in deionized water, and the first and second reactions were carried out sequentially to obtain the ultrathin magnesium-iron ultrastable mineralizer. The roasting temperature is 400~600℃, and the roasting time is 3~6 hours; The iron compound includes ferric acetate and / or ferric citrate; The temperature of the first reaction is 30~60℃, and the time is 1~3 hours; The second reaction is carried out at a temperature of 110~160℃ for 2~6 hours. The reducing gas includes hydrogen or carbon monoxide; The molar ratio of iron in the iron compound to magnesium in magnesium oxide is 1:4 to 1:
2. Application of the ultra-thin magnesium-iron super-stable mineralizer in the remediation of arsenic-contaminated farmland.
2. The preparation method according to claim 1, characterized in that, The dispersion of magnesium oxide and iron compounds in deionized water comprises: dispersing magnesium oxide in deionized water to obtain a magnesium oxide dispersion; dispersing iron compounds in deionized water to obtain an iron compound solution; mixing the magnesium oxide dispersion and the iron compound solution; wherein the concentration of the magnesium oxide dispersion is 0.1~1.2 mol / L; and the concentration of the iron compound solution is 0.025~0.6 mol / L.
3. The preparation method according to claim 1, characterized in that, After the second reaction, the process further includes: separating the obtained second reaction liquid into solid and liquid components, and freeze-drying the obtained solid.
Citation Information
Patent Citations
Method for co-production of synthesis gas by carbonate hydrogenation refining for carbon dioxide emission reduction
CN113582208A
Honeycomb porous Fe / Mg(OH)2 catalytic material and preparation method thereof