Oxidized granular proppant for shale gas reservoir stimulation and preparation and use

By using oxidized particulate proppant with built-in oxidant and slow-release agent in shale gas reservoir stimulation, the problem of insufficient conductivity caused by proppant embedding into the formation or excessive flowback in existing technologies has been solved, achieving efficient stimulation and production increase of shale gas reservoirs.

CN117964397BActive Publication Date: 2026-11-20PETROCHINA CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211314697.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-26
Publication Date
2026-11-20
Estimated Expiration
2042-10-26

AI Technical Summary

Technical Problem

Existing proppants used in shale gas fracturing have problems such as high closure rates or excessively rapid flowback due to embedding in the formation, resulting in insufficient conductivity and affecting the development effect of shale gas.

Method used

Oxidizing particulate proppant with built-in oxidant and slow-release agent is used. The oxidant and slow-release agent are adsorbed by ceramic microspheres, and the oxidant is gradually released in the shale to react with pyrite, forming dissolution cavities and increasing permeability.

Benefits of technology

It significantly improved the conductivity of shale gas reservoirs, enhanced shale gas production, and extended well life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117964397B_ABST
    Figure CN117964397B_ABST
Patent Text Reader

Abstract

The application discloses an oxidized granular proppant for shale gas reservoir reconstruction, characterized in that the proppant is a quartz sand surface film high polymer coating and ceramic microspheres, the ceramic microspheres have honeycomb pores and are filled with oxidants and slow-release agents in the honeycomb pores. In the shale reservoir reconstruction process, the oxidized granular proppant is mixed with other conventional proppants, injected into the formation by means of a fracturing fluid, compacted with the proppant along with the fracture closure, and after the well is shut down, the oxidants are gradually released into the fracture under the control of the slow-release agents, chemically react with pyrite and organic matter in the shale reservoir to produce dissolution cavities, gradually form large voids, and finally achieve the effect of continuously increasing the fracture conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to an oxidized particulate proppant for shale gas reservoir stimulation and its preparation method. Background Technology

[0002] Shale is a fine-grained sediment, typically containing mineral particles smaller than 0.0625 mm. Formed in relatively stable, still water environments, shale is generally dark gray to black in color and is typically a low-porosity, low-permeability reservoir, requiring fracturing for extraction. During fracturing, proppant is continuously injected to support the fractures and prevent formation reclosure, maintaining conductivity and effectively guiding oil and gas into the well, significantly increasing oil and gas production and extending well life. Proppants are made of natural sand or artificial high-strength ceramic particles with a specific particle size and gradation. The surface of the sand or ceramic particles is often coated with resin to further enhance the strength and conductivity of the proppant.

[0003] The inventors discovered that existing proppants suffer from several drawbacks: proppant embedding in the formation leads to high formation end closure rates, or excessively rapid flowback prevents the formation from undergoing repeated fracturing or oxidative fracturing. Current proppants struggle to achieve high conductivity. For example, CN102865061B discloses a honeycomb-type proppant preparation method where some particles are oil-soluble. As crude oil is discharged, the oil-soluble particles dissolve, creating honeycomb-like voids due to the absence of dissolved particles, thus improving fracture conductivity. However, formation migration can cause these voids to collapse, narrowing the fracture and reducing conductivity. CN101121879 discloses a method for preparing oil-soluble powdered ceramic, but the results are not ideal. CN109370557 discloses an oxidation fluid suitable for shale oxidation stimulation; CN110029977 discloses an environmentally friendly oxidation-permeation method for improving oil recovery with zero flowback of fracturing fluid in shale gas wells; CN105626028 proposes a method to increase the fracture network density in shale gas well fracturing stimulation, but all of these suffer from poor oxidation effects due to post-fracturing flowback. CN106701054 discloses a superconducting proppant and its preparation method, but its use suffers from problems such as proppant embedding in the formation and poor end-fracture support capacity.

[0004] The aforementioned problems severely affect the fracture conductivity after shale gas fracturing, thus impacting the effectiveness of shale gas development. Summary of the Invention

[0005] The purpose of this invention is at least to provide a novel shale gas fracturing proppant. This novel proppant carries its own oxidant and slow-release agent. Whether the proppant is embedded in the formation or not, it can slowly release the carried oxidant to oxidize minerals such as pyrite in the nearby shale, thereby gradually increasing the permeability of the shale, improving the conductivity of the shale reservoir, and achieving a significant increase in shale gas production.

[0006] As one aspect of the present invention, an oxidizing particulate proppant for shale gas reservoir stimulation is disclosed, wherein the proppant is a quartz sand surface coated with a polymer coating and ceramic microspheres, the ceramic microspheres having honeycomb pores and being filled with an oxidant and a slow-release agent within the honeycomb pores.

[0007] In one specific embodiment, the proppant is 80-85% quartz sand surface coating, 5-10% polymer coating, and 5-10% ceramic microspheres.

[0008] In one specific embodiment, the ceramic microspheres are formed by mixing powdered alumina with a binder, followed by sintering and granulation, resulting in 30-50 μm particles with honeycomb-like pores. The binder is epoxy resin C. 21 H 23 ClFNO2.

[0009] In one specific embodiment, the polymer coating is a synthetic polymer or a semi-natural / semi-synthetic polymer material, such as phenolic resin C7H6O2.

[0010] In one specific embodiment, the sustained-release agent is nylon 66 (C 36 H 66 N6O6X2); the oxidant is one of calcium peroxide (CaO2) or sodium hypochlorite (NaClO);

[0011] In one specific embodiment, the quartz sand has a particle size of 200-800 μm.

[0012] As another aspect of the present invention, a method for preparing the above-mentioned oxidized particulate proppant for shale gas reservoir stimulation is provided, comprising the following steps:

[0013] 1. Preparation of honeycomb ceramic microspheres: Alumina powder, epoxy resin powder, and epoxy resin curing agent powder are taken in a mass ratio of 20:2:1. Under the conditions of room temperature 20-25℃ and air humidity not exceeding 60%, the alumina powder and epoxy resin powder are poured into a granulator in sequence and mixed evenly. Atomized epoxy resin curing agent solution is continuously sprayed in. The mixture is granulated under the high-speed rotation of the stirring blades. The particles with a diameter of 30-50μm are sieved out and placed in a muffle furnace for high-temperature firing to prepare honeycomb ceramic microspheres with a particle diameter of 30-50μm.

[0014] 2: Adsorption of oxidant and slow-release agent by ceramic microspheres: Pour a saturated mixture of oxidant and slow-release agent into the ceramic microspheres. After the honeycomb particles have fully absorbed the mixture of oxidant and slow-release agent, filter to obtain saturated honeycomb ceramic microspheres and dry them.

[0015] 3. Granulation of finished particle proppant: Honeycomb ceramic microspheres are mixed with quartz sand and granulated at room temperature of 20-25℃ and air humidity not exceeding 60%. Granulation is completed by nitrogen oxygen isolation, two-stage atomized spraying of FFD-301 self-hardening phenolic resin liquid, and two temperature changes to control the viscosity of phenolic resin liquid. The semi-finished oxidized particle proppant with a particle size of 200-800μm of surface-coated phenolic resin and ceramic microspheres is screened out. The semi-finished proppant is then baked and shaped in an oxygen-isolated environment.

[0016] As another aspect of the present invention, it relates to the application of the above-mentioned oxidized particulate proppant for shale gas reservoir stimulation in shale gas reservoir stimulation.

[0017] Compared with existing technologies, this invention proposes the application of ceramic microspheres to adsorb oxidants. The adsorbed oxidants and slow-release agents from these ceramic microspheres are then coated onto the surface of a solid particulate proppant substrate using a water-soluble polymer to create an oxidized particulate proppant. During shale reservoir stimulation, the oxidized particulate proppant is mixed with other conventional proppants and injected into the formation using fracturing fluid. As the fractures close, the proppant is compacted. After well shut-in, the oxidant is gradually released into the fractures under the control of the slow-release agent. It reacts chemically with pyrite and organic matter in the shale reservoir, creating dissolution cavities and gradually forming large voids, ultimately increasing the fracture conductivity. Attached Figure Description

[0018] Figure 1 This is a flowchart illustrating the steps involved in manufacturing the particulate proppant of the present invention.

[0019] Figure 2 Structural diagram of the oxidized particulate proppant according to an embodiment of the present invention;

[0020] Figure 3 A structural diagram of ceramic microspheres according to an embodiment of the present invention. Detailed Implementation

[0021] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are some embodiments of the present invention, but not all embodiments.

[0022] Based on the embodiments of the present invention, those skilled in the art can make several simple modifications and refinements without creative effort, and all other embodiments obtained are within the scope of protection of the present invention.

[0023] Unless otherwise specified, the proportions referred to in this invention are mass ratios.

[0024] The following example illustrates the implementation process of this invention using the preparation of 30kg of solid proppant.

[0025] Natural quartz sand with a diameter of 200-800μm was selected as the substrate for the solid proppant, with a sphericity greater than 0.8 and a roundness greater than 0.8.

[0026] Fabrication of ceramic microspheres: Under conditions of room temperature 20-25℃ and air humidity not exceeding 60%, 20 kg of 5-10 μm alumina powder (#2000# mesh alumina powder produced by Zhengzhou Haixu Abrasives Co., Ltd.) and 2 kg of 5-10 μm epoxy resin powder (such as SH-E55 series ultrafine epoxy resin powder produced by Guangzhou Xinxi Metallurgical Chemical Co., Ltd.) are sequentially poured into a small mixing granulator (such as Qingdao Sentaike Electromechanical Technology Co., Ltd.). After stirring for 20 minutes to ensure uniform mixing, the granulator speed is adjusted to control the particle size, while continuously spraying atomized... One kg of epoxy resin curing agent solution (such as CYDHD-593 epoxy resin curing agent produced by China Petroleum & Chemical Corporation) is granulated in a granulator under the combined action of a high-speed rotor, granulation disc, and multi-functional scraper for 1 hour. The granules are then sieved, and the granules with a diameter of 30-50 μm are placed in a muffle furnace (such as a Fisford SX4-7-12P ceramic fiber muffle furnace) and fired at 900℃ for 30 minutes to remove the epoxy resin and curing agent and other organic components, thus preparing honeycomb ceramic microspheres with a diameter of 30-50 μm. These microspheres are then dried in a dryer for later use.

[0027] Preparation of a saturated oxidant and slow-release agent mixed solution: Pour 2 kg of calcium peroxide (oxidant), 0.5 kg of sodium benzoate (bactericide), and 0.5 kg of nylon 66 (slow-release agent, such as products from Shenma Industrial Co., Ltd.) into a container containing 25 L of water, while stirring continuously for 2 hours until a small amount of solid residue remains at the bottom of the solution, indicating that the solution has reached saturation. After standing for 2 hours, filter the mixture to remove the residue and set aside for later use, thus preparing a milky white mixed solution of saturated oxidant and slow-release agent for the next step.

[0028] Adsorption of oxidant and slow-release agent by granular ceramic microspheres: A prepared mixed solution of oxidant and slow-release agent is introduced into the ceramic microspheres and stirred continuously for 2-4 minutes to ensure thorough mixing of the oxidant and slow-release agent solution with the honeycomb ceramic microsphere particles. After standing for 12 hours, the honeycomb particles are allowed to fully absorb the oxidant solution. The saturated honeycomb ceramic microspheres are then filtered and placed in a dry, sealed container. The sealed container is continuously purged with nitrogen gas at a temperature not lower than 90°C for rinsing and drying. The ceramic microspheres are then immersed in the oxidant solution again for adsorption, filtered again, dried, and placed in a nitrogen-filled sealed container for later use.

[0029] Granulation of the particle proppant: Dry natural quartz sand and honeycomb ceramic microspheres are added sequentially to a small stirred granulator at a weight ratio of 50:1 for granulation. Under ambient conditions of 20-25℃ and air humidity not exceeding 60%, the natural quartz sand is first placed into the granulation chamber, and the chamber temperature is raised to 60℃. While stirring, FFD-301 self-hardening phenolic resin liquid (such as products from Chengdu Huaxia Chemical Reagent Co., Ltd.) is sprayed into the granulator chamber via atomization at a flow rate of approximately 200ml / min. After stirring for 20 minutes, the phenolic resin is uniformly adhered to the surface of the natural quartz sand. Then, the granulator is turned on, and the ceramic microspheres are poured in all at once to begin granulation. Simultaneously, nitrogen gas is introduced into the granulation chamber for flushing to reduce oxidation, and the chamber temperature is raised to approximately 100℃ to increase the phenolic resin content. The viscosity of the resin liquid is adjusted to allow the natural gas quartz sand to adhere to the ceramic microspheres. After granulation for 30 minutes, the surface of the natural gas quartz sand is almost completely covered with ceramic microspheres. Then, FFD-301 self-hardening phenolic resin liquid is sprayed into the granulation chamber at a flow rate of about 100 ml / min for 10 minutes to finish granulation, forming an oxidized particulate proppant semi-finished product (quartz sand surface coated with phenolic resin and ceramic microspheres). Particles with a particle size of 200-800 μm are sieved out and placed in an oven. Nitrogen gas is introduced to isolate oxygen, and the proppant sample with the self-hardening phenolic resin on the surface is shaped at a temperature of 188℃ to produce the finished particulate proppant product.

[0030] The properties of the prepared proppant were tested.

[0031] 1. Testing the roundness and sphericity of the proppant

[0032] Sphericity is a measure of the degree of approximation to a spherical shape. Roundness is a measure of the sharpness of the proppant particle angles. For each particle size, 5 to 15 g of proppant sample was selected and laid flat. The sample was observed using a low-magnification microscope (10 to 40x). At least 20 samples were randomly selected, and their sphericity and roundness were recorded and averaged. As shown in Table 1, the roundness and sphericity of the proppant of this invention are both greater than 0.8, exhibiting excellent sphericity and roundness performance, which can support the flow of formation fluids.

[0033] Table 1: Results of sphericity and roundness tests for oxidized particulate proppant

[0034] Particle size specification / μm sphericity Roundness 600-800 0.91 0.85 400-600 0.85 0.86 200-400 0.86 0.88

[0035] 2. Testing the coating effect of particulate proppant

[0036] To test the coating effect of quartz sand, a small amount of quartz sand can be randomly selected and calcined in a high-temperature muffle furnace to test the coating quality. The coating mass ratio should not be less than 3%. Weigh 5-8g of the coating support sample using an analytical balance and place it in a crucible. Cover the crucible and place it in a muffle furnace at 900℃ for 2 hours to remove the polymer coating using a combustion method. Transfer the covered crucible and sample to a desiccator to cool to room temperature. Weigh the remaining support material using an analytical balance. The difference before and after calcination is the coating mass, as shown in Table 2. The coating mass of this product is greater than 3%, meeting the product's technical requirements. If other polymer coating materials are used, the weight used will differ from that used with phenolic resin. The weight ratio of ceramic microspheres to coating polymer material should be adjusted experimentally to ensure that the coating mass ratio is not less than 3%.

[0037] Table 2: High-temperature ignition test results of samples with different particle sizes

[0038]

[0039]

[0040] 3. Testing the supporting effect of particulate proppant

[0041] The technical requirements for finished granular proppant are that the proppant remains stable under stress of 30-60 MPa and the breakage rate is less than 5% under stress of 90 MPa. Three identical proppant samples, each weighing 5 g, were taken for each particle size. The samples were spread evenly in a crushing chamber, which was then placed in a standard single-shaft hydraulic press. Pressure was applied to 30 MPa, 60 MPa, and 90 MPa respectively, and after 2 minutes of pressurization, the samples were removed, sieved, and the breakage rate was calculated. The test results are shown in Table 3.

[0042] Table 3: Breakage rate test results of samples with different particle sizes

[0043]

[0044] The proppant of this invention remains stable under stress of 30-60 MPa and has a breakage rate of less than 5% under stress of 90 MPa, thus maintaining stability under high pressure during fracturing.

[0045] 4. Comparative Test of Propion Support Effect

[0046] Using an analytical balance, 10g of ordinary quartz sand (200-800μm) and 10g of oxidant-type particulate proppant (200-800μm) prepared according to this invention were weighed separately, and a comparative experiment on the fracturing propping effect was conducted. The shale fracturing physical simulation device was activated, with a maximum operating pressure of 70MPa and a simulated temperature of 150℃. First, a confining pressure of 30MPa was applied to the shale sample to simulate underground pressure conditions. A mixture of slickwater and 200-800μm proppant was injected into the shale sample at a pressure of 35MPa. The experiment lasted 1-2 hours. Then, the shale sample was removed, and the shale was cut open using a wire cutting method to observe the fracture density distribution per unit length (see Table 5). Simultaneously, two 2.54cm diameter plunger samples were drilled from the shale after the fracturing experiment to test porosity and permeability. The test results were averaged (see Table 4).

[0047] Table 4: Comparative Experimental Results of Shale Samples from the Present Invention and Ordinary Quartz Sand Samples

[0048]

[0049]

[0050] The comparison of the above experimental results shows that the number of fractures in the shale after fracturing with the proppant of the present invention is significantly greater than that of ordinary quartz sand. The porosity of the shale reaches 4.5%, and the permeability reaches 0.21541 md, both of which are significantly higher than the control group. The porosity of the shale is increased by 35%, and the permeability is increased by 15 times, proving that the proppant of the present invention has good implementation effect.

[0051] The present invention has been described above in conjunction with specific features and embodiments. It is obvious that various modifications and combinations can be made without departing from the spirit and scope of the invention. Accordingly, this specification and accompanying drawings are merely exemplary descriptions of the invention as defined by the appended claims, and are considered to cover any and all modifications, variations, combinations, or equivalents within the scope of the invention. Clearly, those skilled in the art can make various alterations and modifications to the present invention, and these modifications and modifications that do not depart from the spirit and scope of the invention also fall within the scope of the claims and their equivalents.

Claims

1. An oxidized particulate proppant for shale gas reservoir stimulation, characterized in that, The proppant is a quartz sand surface-coated polymer coating and ceramic microspheres. The ceramic microspheres have honeycomb pores and are filled with oxidant and slow-release agent. The ceramic microspheres are formed by mixing powdered alumina with a binder, followed by granulation and firing, resulting in 30-50 μm particles with honeycomb-like pores. The sustained-release agent is nylon 66; the oxidant is calcium peroxide.

2. The oxidized particulate proppant for shale gas reservoir stimulation as described in claim 1, characterized in that, The proppant consists of 80-85% quartz sand surface coating, 5-10% polymer coating, and 5-10% ceramic microspheres.

3. The oxidized particulate proppant for shale gas reservoir stimulation as described in claim 1, characterized in that, The quartz sand has a particle size of 200-800μm.

4. A method for preparing the oxidized particulate proppant for shale gas reservoir stimulation as described in any one of claims 1-3, characterized in that, Includes the following steps: 1) Preparation of honeycomb ceramic microspheres: Alumina powder, epoxy resin powder and epoxy resin curing agent powder are taken in a mass ratio of 20:2:

1. Under the conditions of room temperature 20-25℃ and air humidity not exceeding 60%, the alumina powder and epoxy resin powder are poured into a granulator in sequence and mixed evenly. Atomized epoxy resin curing agent solution is continuously sprayed in to mix and granulate. The mixture is then placed in a muffle furnace for high-temperature firing to prepare honeycomb ceramic microspheres. 2) Adsorption of oxidant and slow-release agent by ceramic microspheres: Pour a saturated mixture of oxidant and slow-release agent into the ceramic microspheres. After the honeycomb particles have fully absorbed the mixture of oxidant and slow-release agent, filter to obtain saturated adsorption honeycomb particles of ceramic microspheres and dry them. 3) Granulation of finished particle proppant: Honeycomb ceramic microspheres are mixed with quartz sand and granulated at room temperature of 20-25℃ and air humidity not exceeding 60%. Granulation is completed by nitrogen oxygen isolation, two-stage atomized spraying of FFD-301 self-hardening phenolic resin liquid, and two temperature changes to control the viscosity of phenolic resin liquid. The semi-finished oxidized particle proppant with a particle size of 200-800μm of surface-coated phenolic resin and ceramic microspheres is screened out and the semi-finished proppant is baked and shaped in an oxygen-isolated environment.

5. The method according to claim 4, characterized in that, include: The particles, with a diameter of 30-50 μm, are fired at high temperature in a muffle furnace to prepare honeycomb ceramic microspheres with a particle diameter of 30-50 μm.

6. The application of the oxidized particulate proppant according to any one of claims 1-3 in shale gas reservoir stimulation.

Citation Information

Patent Citations

  • Honeycomb laying method and application of proppant

    CN102865061B

  • Coating support agent with sustained release and gel breaking effect on fracturing fluid and preparation method of coating support agent

    CN110055048A

  • Kaolin ceramic microsphere, preparation method thereof, and application of kaolin ceramic microsphere in heat-conducting filler

    CN111363202A

  • Increasing Fracture Complexity in Ultra-Low Permeable Subterranean Formation Using Degradable Particulate

    US20120024530A1