A method for producing pyromellitic acid by liquid phase oxidation

By using a metal-organic framework catalyst encapsulating cobalt and manganese in pyromellitic acid, the active metal is encapsulated in the liquid-phase oxidation reaction, solving the problems of waste liquid corrosion and the difficulty in reusing the catalyst in the liquid-phase oxidation method, and realizing the efficient production of high-purity pyromellitic acid.

CN117964477BActive Publication Date: 2026-11-24CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211319076.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-26
Publication Date
2026-11-24
Estimated Expiration
2042-10-26

AI Technical Summary

Technical Problem

Existing liquid-phase oxidation methods suffer from waste liquid corrosion and pollution problems in homogeneous catalysis, and the catalyst is difficult to reuse, resulting in low product purity and difficult treatment.

Method used

A metal-organic framework catalyst encapsulating cobalt and manganese in pyromellitic acid is used to carry out an oxidation reaction in a liquid solution. The target product is used as an organic framework to encapsulate the active metal, which reduces the influence of organic impurities and enables the catalyst to be reused multiple times.

Benefits of technology

The conversion rate of the product mesitylene and the selectivity of pyromellitic acid reached over 90%. The catalyst was pollution-free and could be reused multiple times, solving the problems of waste liquid corrosion and treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117964477B_ABST
    Figure CN117964477B_ABST
Patent Text Reader

Abstract

This invention discloses a method for producing pyromellitic acid via liquid-phase oxidation. The method includes: reacting mesitylene with an oxygen-containing gas in a liquid solution in the presence of a metal-organic framework catalyst encapsulating cobalt and manganese in pyromellitic acid. By using the target product as an organic framework to encapsulate the active metal, the method significantly reduces the impact of other organic impurities on product purity. Furthermore, compared to traditional homogeneous liquid-phase catalysis which requires highly corrosive Br ions and other transition metals, leading to difficulties in subsequent wastewater treatment, this invention allows for multiple reuses of the catalyst without pollution, and achieves a conversion rate of over 90% for the target product mesitylene and a selectivity for pyromellitic acid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for producing pyromellitic acid by liquid-phase oxidation. Background Technology

[0002] Pyromellitic acid (1,2,4,5-phenylenetetracarboxylic acid, PMA) is an important organic intermediate widely used in the preparation of various high-end fine materials. The dehydration product of pyromellitic acid is pyromellitic dianhydride (1,2,4,5-phenylenetetracarboxylic dianhydride, PMDA), which is one of the important precursors for the synthesis of polyimide (PI). Polyimide is a special polymer material with advantages such as wide operating temperature, chemical resistance, and high strength. DuPont first launched commercial polyimide in 1961. Since then, polyimide, as a special engineering material, has been widely used in aerospace, microelectronics, nanotechnology, liquid crystals, separation membranes, lasers, and other fields.

[0003] PMDA synthesis methods generally involve the oxidation of mesitylene (1,2,4,5-tetramethylbenzene), which can be further divided into gas-phase and liquid-phase methods. The gas-phase method primarily uses tubular reactors and supported catalysts, reacting at high temperatures of 350-450℃, achieving a PMDA molar yield of approximately 50-60%. The liquid-phase method uses oxidizing acids (nitric acid) or transition metal / bromine systems, with reaction temperatures around 170-240℃, achieving a PMA molar yield of 70-80%, followed by dehydration upon heating to produce PMDA. The advantage of the gas-phase method is its one-step direct synthesis of PMDA and the use of a heterogeneous catalyst. However, due to the high reaction temperature, it produces many byproducts, resulting in lower product purity, and PMDA still needs to be hydrolyzed back to PMA for further purification. The liquid-phase method, on the other hand, has a moderate reaction temperature, and its conversion rate and selectivity are much higher than the gas-phase method. However, the homogeneous reaction system contains highly corrosive nitric acid and bromine elements, placing high demands on reactor selection.

[0004] Amoco Inc. published US 5041633 (Process for the Production of An Aromatic Polycarboxylic Acid), dated August 20, 1991, which describes a method for preparing pyromellitic acid (PMA). This method utilizes a Co-Mn-Br homogeneous catalyst to catalytically oxidize mesitylene to PMA. The PMA yield is approximately 80%, but issues regarding catalyst recovery and equipment corrosion remain unresolved. Summary of the Invention

[0005] The purpose of this invention is to overcome the problem of waste liquid corrosion and pollution in the existing homogeneous oxidation process and to provide a new green and efficient liquid-phase oxidation method for producing pyromellitic acid. This method has the advantages of high product yield, no corrosive waste liquid and no metal loss.

[0006] To achieve the above objectives, the present invention provides a method for producing pyromellitic acid by liquid-phase oxidation, the method comprising: oxidizing pyromellitic acid with an oxygen-containing gas in a liquid solution in the presence of a metal-organic framework catalyst containing cobalt and manganese encapsulated in pyromellitic acid.

[0007] By using the above technical solution, the target product is used as an organic framework to encapsulate the active metal. On the one hand, this completely reduces the impact of other organic impurities on product purity. On the other hand, compared with the traditional homogeneous liquid-phase catalysis which requires highly corrosive Br ions and other transition metals, resulting in difficulties in subsequent waste liquid treatment, the method of this invention enables the catalyst to be reused multiple times without pollution, and the conversion rate of the target product pyromellitic acid and the selectivity of pyromellitic acid can reach more than 90%. Attached Figure Description

[0008] Figure 1 The image shows the Raman spectra of the Co / Mn organic framework material encapsulated in pyromellitic acid from Example 1 and pyromellitic acid. Detailed Implementation

[0009] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0010] This invention provides a method for producing pyromellitic acid via liquid-phase oxidation. The method includes: reacting mesitylene with an oxygen-containing gas in a liquid solution in the presence of a metal-organic framework catalyst encapsulating cobalt and manganese in pyromellitic acid. This invention uses the target product as an organic framework to encapsulate the active metal, which on the one hand completely reduces the impact of other organic impurities on product purity; on the other hand, compared to traditional homogeneous liquid-phase catalysis which requires highly corrosive Br ions and other transition metals, resulting in difficulties in subsequent wastewater treatment.

[0011] In this invention, the molar ratio of pyromellitic acid to metal can be selected within a wide range. According to a preferred embodiment of the invention, in the pyromellitic acid-encapsulated cobalt and manganese metal-organic framework catalyst, the molar ratio of pyromellitic acid to metal is 0.5–10, preferably 1–9, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, etc. By adopting the aforementioned preferred embodiment, the catalyst can be reused multiple times without pollution, and the conversion rate of the target product, pyromellitic acid, and the selectivity of pyromellitic acid can reach over 90%.

[0012] In this invention, the molar ratio of cobalt to manganese has a wide selectable range. For this invention, the preferred molar ratio of cobalt to manganese is 0.1–10, more preferably 0.5–2, for example 0.2, 0.4, 0.6, 0.8, 1.0, 1.2, 1.4, 1.6, 1.8, 2, 2.2, 2.4, 2.6, 2.8, 3.0, 3.2, 3.4, 3.6, 3.8, 4, 5.2, etc. By employing the aforementioned preferred embodiments, the catalyst can be reused multiple times without pollution, and the conversion rate of the target product, pyromellitic acid, and the selectivity can reach over 90%.

[0013] The metal-organic framework catalyst of the present invention can achieve the purpose of the present invention as long as it has the aforementioned composition, and there are no special requirements for its preparation method. For the present invention, the preferred preparation method of the metal-organic framework catalyst of cobalt and manganese encapsulated by pyromellitic acid includes: pyromellitic acid reacting with cobalt salt and manganese salt in a polar solvent in a solvothermal reaction, separating the solid and liquid to obtain a solid product, and then drying it.

[0014] In this invention, the drying conditions can be selected from a wide range. For this invention, the preferred drying conditions include a temperature of 50–150°C, preferably 80–120°C. The drying time is determined as needed, for example, 4–8 hours.

[0015] In this invention, the range of conditions for the solvothermal reaction is relatively wide. For this invention, the preferred conditions for the solvothermal reaction include: a temperature of 100-200°C, preferably 130-170°C, for example 130°C, 140°C, 150°C, 160°C, and 170°C.

[0016] The solvothermal reaction time in this invention has a wide range of selectable values. For this invention, the preferred solvothermal reaction time is 1-10 hours, and more preferably 4-8 hours.

[0017] In this invention, the molar ratio of pyromellitic acid to polar solvent in the solvothermal reaction can be selected within a wide range. For this invention, the preferred molar ratio of pyromellitic acid to polar solvent is 0.05 to 2, more preferably 0.2 to 1.8, for example 0.2, 0.4, 0.6, 0.8, 1.0, 1.2, 1.4, 1.6, 1.8.

[0018] In this invention, the range of cobalt salts that can be selected is relatively wide. For this invention, it is preferred that the cobalt salt be selected from one or more of cobalt acetate, cobalt oxalate, cobalt chloride and cobalt nitrate, with cobalt acetate being the most preferred.

[0019] In this invention, the range of types of manganese salts is relatively wide. For this invention, the manganese salt is preferably selected from one or more of manganese acetate, manganese oxalate, manganese chloride, and manganese nitrate, with manganese acetate being the most preferred.

[0020] In this invention, the range of types of polar solvents is relatively wide. For this invention, the polar solvent is preferably selected from one or more of N,N-dimethylformamide, N-methylpyrrolidone and dimethyl sulfoxide, with N,N-dimethylformamide being more preferred.

[0021] According to a preferred embodiment of the present invention, the synthesis process of the metal-organic framework catalyst includes: a solvothermal reaction of pyromellitic acid with cobalt acetate and manganese acetate in N,N-dimethylformamide, followed by solid-liquid separation to obtain a solid product, and then drying.

[0022] In this invention, the mass ratio of the metal-organic framework catalyst to mesitylene can be selected within a wide range. For this invention, the preferred mass ratio of the metal-organic framework catalyst to mesitylene is 0.05 to 0.5, and more preferably 0.1 to 0.3.

[0023] In this invention, the conditions for the oxidation reaction can be selected from a wide range. For this invention, the preferred temperature for the oxidation reaction is 120-270°C, preferably 180-220°C, for example 180°C, 190°C, 200°C, 210°C, or 220°C.

[0024] In this invention, the conditions for the oxidation reaction can be selected over a wide range. For this invention, the preferred pressure for the oxidation reaction is 10 to 30 bar, for example, 10 bar, 20 bar, or 30 bar.

[0025] In this invention, the conditions for the oxidation reaction can be selected from a wide range. For this invention, the preferred oxidation reaction time is 60 to 150 min, for example, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, or 120 min.

[0026] In this invention, the range of liquid solvents that can be selected for the oxidation reaction is relatively wide, and there are no special requirements for this. For this invention, the preferred liquid solvent for the oxidation reaction is one or more of acetic acid, water, and acetic anhydride, with acetic acid being the most preferred.

[0027] In this invention, there are no special requirements for the oxygen-containing gas; for example, it can be air.

[0028] According to the present invention, a preferred method of the present invention comprises: mixing mesitylene and a liquid solvent, then adding an organic framework catalyst, and heating to a first temperature and a first pressure at a rate of 1-5 °C / min under an inert atmosphere; then introducing oxygen-containing gas at a rate of 1-50 L / min, and heating to the oxidation reaction temperature at a rate of 2-10 °C / min to carry out the oxidation reaction.

[0029] According to the present invention, preferably, the first temperature is 130-150°C and the first pressure is 10-20 bar. This is well known to those skilled in the art, and will not be described in detail here.

[0030] According to the present invention, preferably, the method further includes: after the oxidation reaction is completed, cooling the filtrate to crystallize and drying the solid to obtain pyromellitic acid. This is well known to those skilled in the art, and will not be described in detail here.

[0031] By using the above technical solution, the target product is used as an organic framework to encapsulate the active metal. On the one hand, this completely reduces the impact of other organic impurities on product purity. On the other hand, compared with the traditional homogeneous liquid-phase catalysis which requires highly corrosive Br ions and other transition metals, resulting in difficulties in subsequent waste liquid treatment, the method of this invention enables the catalyst to be reused multiple times without pollution, and the conversion rate of the target product pyromellitic acid and the selectivity of pyromellitic acid both exceed 90%.

[0032] The present invention will be described in detail below through embodiments. In the following embodiments,

[0033] The conversion rate of mesitylene and the selectivity parameters of pyromellitic acid were obtained by measuring the concentrations of mesitylene and pyromellitic acid using liquid chromatography (GC 780) and then calculating them. The method is as follows: The concentration parameter of pyromellitic acid was measured by comparing the integral area of ​​a pyromellitic acid standard (99.9 wt%, Sinopharm) using liquid chromatography (GC 780); the raw material of mesitylene was a commercially available product from Wokai Company with the brand name XW9593202.

[0034] Example 1

[0035] 0.5 mol of cobalt acetate, 0.5 mol of manganese acetate, and 1 mol of pyromellitic acid were added to 5 mol of N,N-dimethylformamide solvent and stirred until homogeneous. The mixture was reacted in a sealed hydrothermal reactor at 150 °C for 6 h. The mixture was then filtered, and the solid was dried in an oven at 100 °C for 6 h, and designated as Co-Mn-Pyro-MOF.

[0036] The Raman spectrum of the catalyst Co-Mn-Pyro-MOF is shown below. Figure 1 , Figure 1 This indicates that Co and Mn metal ions react with pyromellitic acid at a concentration of 1250-1450 cm⁻¹. -1 The presence of a distinct characteristic peak compared to pyromellitic acid indicates that the Co-Mn bimetallic compound forms a metal-organic framework material with pyromellitic acid.

[0037] 100 g of mesitylene (98 wt.%) was added to 400 g of acetic acid solvent and stirred until homogeneous. Then, 2.5 g of Co-Mn-Pyro-MOF was added. The temperature in the stirred tank was gradually increased to 140 °C over 50 min, while nitrogen gas was introduced to maintain a pressure of 20 bar. Simultaneously, air was introduced at a rate of 10 L / min, and the temperature in the stirred tank was raised to 200 °C and the pressure increased to 30 bar. The reaction was carried out for 2 h. The reaction solution was filtered while hot to remove solid impurities and catalyst. The filtrate was cooled at 15 °C to crystallize, and the filtered solid was then dried in an oven at 100 °C for 6 h to obtain pyromellitic acid (PMA) product. The conversion rate of mesitylene was 87.4 mol.%, and the selectivity of PMA was 90.3 mol.%.

[0038] Example 2

[0039] 0.5 mol of cobalt acetate, 0.5 mol of manganese acetate, and 3 mol of pyromellitic acid were added to 5 mol of N,N-dimethylformamide solvent and stirred until homogeneous. The mixture was reacted in a sealed hydrothermal reactor at 150 °C for 6 h. The mixture was then filtered, and the solid was dried in an oven at 100 °C for 6 h, and designated as Co-Mn-Pyro-2-MOF.

[0040] 100 g of mesitylene (98 wt.%) was added to 400 g of acetic acid solvent and stirred until homogeneous. Then, 2.5 g of Co-Mn-Pyro-2-MOF was added. The temperature in the stirred tank was gradually increased to 140 °C over 50 min, while nitrogen gas was introduced to maintain a pressure of 20 bar. Simultaneously, air was introduced at a rate of 10 L / min, and the temperature in the stirred tank was raised to 200 °C and the pressure increased to 30 bar. The reaction was carried out for 2 h. The reaction solution was filtered while hot to remove solid impurities and catalyst. The filtrate was cooled at 15 °C to crystallize, and the filtered solid was then dried in an oven at 100 °C for 6 h to obtain pyromellitic acid (PMA) product. The conversion rate of mesitylene was 90.1 mol.%, and the selectivity of PMA was 95.6 mol.%.

[0041] Example 3

[0042] 0.5 mol of cobalt acetate, 0.5 mol of manganese acetate, and 9 mol of pyromellitic acid were added to 5 mol of N,N-dimethylformamide solvent and stirred until homogeneous. The mixture was reacted in a sealed hydrothermal reactor at 150 °C for 6 h. The mixture was then filtered, and the solid was dried in an oven at 100 °C for 6 h, and designated as Co-Mn-Pyro-3-MOF.

[0043] 100 g of mesitylene (98 wt.%) was added to 400 g of acetic acid solvent and stirred until homogeneous. Then, 2.5 g of Co-Mn-Pyro-3-MOF was added. The temperature in the stirred tank was gradually increased to 140 °C over 50 min, while nitrogen gas was introduced to maintain a pressure of 20 bar. Simultaneously, air was introduced at a rate of 10 L / min, and the temperature in the stirred tank was raised to 200 °C and the pressure increased to 30 bar. The reaction was carried out for 2 h. The reaction solution was filtered while hot to remove solid impurities and catalyst. The filtrate was cooled at 15 °C to crystallize, and the filtered solid was then dried in an oven at 100 °C for 6 h to obtain pyromellitic acid (PMA) product. The conversion rate of mesitylene was 80.9 mol.%, and the selectivity of PMA was 85.2 mol.%.

[0044] Example 4

[0045] The method of Example 3 was followed, except that the molar amount of pyromellitic acid was 15 mol. The results are shown in Table 1.

[0046] Example 5

[0047] The method of Example 2 was followed, except that 0.1 mol of cobalt acetate and 0.9 mol of manganese acetate were used, while the other conditions remained the same. The results are shown in Table 1.

[0048] Example 6

[0049] The method of Example 2 was followed, except that the polar solvent was N-methylpyrrolidone. The results are shown in Table 1.

[0050] Comparative Example 1

[0051] 100 g of mesitylene (98 wt.%) was added to 400 g of acetic acid solvent and stirred until homogeneous. Then, 0.5 mol of cobalt acetate, 0.5 mol of manganese acetate, and 1 mol of pyromellitic acid were added. The mixture was gradually heated to 140 °C over 50 min while nitrogen gas was introduced, maintaining a pressure of 20 bar. Simultaneously, air was introduced at a rate of 10 L / min, and the mixture was heated again to 200 °C and the pressure increased to 30 bar. The reaction was carried out for 2 h. The reaction solution was filtered while hot to remove solid impurities and catalyst. The filtrate was cooled at 15 °C to crystallize, and the filtered solid was then dried in an oven at 100 °C for 6 h to obtain pyromellitic acid (PMA) product. The mesitylene conversion rate was 40.2 mol.%, and the PMA selectivity was 4.5 mol.%.

[0052] Table 1

[0053]

[0054]

[0055] If the data in the table differs from the example, the example shall prevail.

[0056] As can be seen from the results in Table 1, the method of the present invention has significantly better results in terms of pyromellitic acid conversion rate and selectivity.

[0057] The method of this invention uses the target product as an organic framework to encapsulate the active metal. On the one hand, it completely reduces the impact of other organic impurities on product purity. On the other hand, compared with the traditional homogeneous liquid-phase catalysis, which requires highly corrosive Br ions and other transition metals, resulting in difficulties in subsequent waste liquid treatment, the method of this invention enables the catalyst to be reused multiple times without pollution, and the conversion rate of the target product pyromellitic acid and the selectivity of pyromellitic acid can reach more than 90%.

[0058] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A process for the liquid phase oxidation production of pyromellitic acid, characterized in that, The method includes: In the presence of a metal-organic framework catalyst containing cobalt and manganese encapsulated in pyromellitic acid, the oxidation reaction of pyromellitic acid with oxygen-containing gas is completed in a liquid solution.

2. The method of claim 1, wherein, In the metal-organic framework catalyst encapsulated with pyromellitic acid for cobalt and manganese: The molar ratio of pyromellitic acid to metal is 0.5~10; and / or The molar ratio of cobalt to manganese is 0.1 to 10.

3. The method of claim 2, wherein, In the metal-organic framework catalyst encapsulated with pyromellitic acid for cobalt and manganese: The molar ratio of pyromellitic acid to metal is 1~9; and / or The molar ratio of cobalt to manganese is 0.5 to 2.

4. The method according to any one of claims 1-3, wherein, The preparation methods of cobalt and manganese metal-organic framework catalysts encapsulated in pyromellitic acid include: Pyromellitic acid undergoes a solvothermal reaction with cobalt and manganese salts in a polar solvent, followed by solid-liquid separation to obtain a solid product, which is then dried.

5. The method according to claim 4, wherein, The drying conditions include: a temperature of 50~150 ℃; and / or a time of 4~8 h; and / or The conditions for a solvothermal reaction include: Temperature: 100~200℃; Time: 1-10 h; and / or The molar ratio of pyromellitic acid to polar solvent is 0.05~2.

6. The method according to claim 5, wherein, Drying conditions include a temperature of 80-120℃; and / or The conditions for a solvothermal reaction include: Temperature: 130-170℃; Time: 4-8 hours; and / or The molar ratio of pyromellitic acid to polar solvent is 0.2~1.

8.

7. The method according to claim 4, wherein, The cobalt salt is selected from one or more of cobalt acetate, cobalt oxalate, cobalt chloride, and cobalt nitrate; and / or The manganese salt is selected from one or more of manganese acetate, manganese oxalate, manganese chloride, and manganese nitrate; and / or The polar solvent is selected from one or more of N,N-dimethylformamide, N-methylpyrrolidone, and dimethyl sulfoxide.

8. The method according to claim 7, wherein, The cobalt salt is cobalt acetate; and / or The manganese salt is manganese acetate; and / or The polar solvent is N,N-dimethylformamide.

9. The method according to claim 8, wherein, The synthesis process of metal-organic framework catalysts includes: a solvothermal reaction of pyromellitic acid with cobalt acetate and manganese acetate in N,N-dimethylformamide, followed by solid-liquid separation to obtain a solid product, which is then dried.

10. The method of claim 1, wherein, The mass ratio of the metal-organic framework catalyst to mesitylene is 0.05~0.

5.

11. The method of claim 10, wherein, The mass ratio of the metal-organic framework catalyst to mesitylene is 0.1 to 0.

3.

12. The method of claim 1, wherein, The oxidation reaction temperature is 120~270℃; and / or The pressure for the oxidation reaction is 10~30 bar.

13. The method of claim 12, wherein, The oxidation reaction takes place at a temperature of 180-220℃.

14. The method of claim 1, wherein, The oxidation reaction takes 60 to 150 minutes.

15. The method according to claim 1, wherein, The liquid solvent for the oxidation reaction is one or more of acetic acid, water, and acetic anhydride; and / or The oxygen-containing gas is air; The method includes: mixing mesitylene and a liquid solvent, then adding an organic framework catalyst, and heating to a first temperature and a first pressure at a rate of 1-5 °C / min under an inert atmosphere, wherein the first temperature is 130-150 °C and the first pressure is 10-20 bar. Then, oxygen-containing gas is introduced at a rate of 1-50 L / min, and the temperature is increased to the oxidation reaction temperature at a rate of 2-10 °C / min to carry out the oxidation reaction. The method also includes: after the oxidation reaction is completed, the filtrate is cooled and crystallized, and the solid is dried to obtain pyromellitic acid.

16. The method according to claim 15, wherein, The liquid solvent for the oxidation reaction is acetic acid.

Citation Information

Patent Citations

  • Process for the production of an aromatic polycarboxylic acid

    US5041633A

  • Method for producing pyromellitic dianhydride by low-temperature liquid-phase continuous oxidation of durene

    CN110746435A

  • Method for synthesizing pyromellitic dianhydride through durene liquid-phase continuous oxygen-enriched precise oxidation

    CN113583014A