Superfine heat treatment method for improving toughness of hot work die steel and preparation method thereof

By using ultra-fine heat treatment methods, including ultra-fine refining, tempering, and spheroidizing annealing, the microstructure of hot work die steel is optimized, solving the problem of insufficient toughness in large-size die steel and significantly improving the strength and toughness of the die.

CN117965850BActive Publication Date: 2026-11-24CHENGDU ADVANCED METAL MATERIALS IND TECH RES INST CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410183365.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-19
Publication Date
2026-11-24
Estimated Expiration
2044-02-19

AI Technical Summary

Technical Problem

Existing hot work die steels lack toughness when used under high temperature and high pressure conditions. In particular, large-size die steels suffer from severe component segregation and poor microstructure uniformity, which affects their service life.

Method used

An ultra-fine heat treatment method is adopted, including ultra-fine treatment, tempering treatment and spheroidizing annealing treatment. The parameters of each process are controlled, and the microstructure is optimized by segmented cooling to promote the dispersion and precipitation of carbides.

Benefits of technology

It effectively controls the austenite grain size, improves the strength and toughness of hot work die steel, and extends the service life of dies, especially significantly improving the toughness of large-size dies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117965850B_ABST
    Figure CN117965850B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of iron and steel metallurgy technology, and discloses an ultrafine heat treatment method for improving the toughness of hot work die steel and a method for preparing high-toughness hot work die steel. The ultrafine heat treatment method includes: ultrafine treatment of forged billets at a holding temperature of 1020–1080℃ for 30–90 min; tempering of the ultrafine-treated billets at a tempering temperature of 550–600℃ for 1–2 h; and spheroidizing annealing of the tempered billets to obtain finished steel at a spheroidizing annealing temperature of 840–860℃ for 1–3 h. This method effectively controls the austenite grain size and promotes dispersed carbide precipitation, thereby improving the strength and toughness of hot work die steel and extending the service life of the dies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of iron and steel metallurgy technology, specifically relating to an ultra-fine heat treatment method for improving the toughness of hot work die steel and a method for preparing high-toughness hot work die steel. Background Technology

[0002] Hot work die steel refers to alloy tool steel suitable for making dies for hot deformation of metals, such as hot forging dies, hot extrusion dies, die casting dies, and hot upsetting dies. Because hot work dies operate under high temperature and high pressure conditions for extended periods, the die material is required to have high strength, hardness, and thermal stability, especially high thermal strength, resistance to thermal fatigue, toughness, and wear resistance.

[0003] Hot work die steels operate in harsh environments, experiencing rapid temperature fluctuations that create significant temperature differences between the inside and outside of the die, generating intense stress and demanding high toughness. Furthermore, as the size of the die steel increases, noticeable compositional segregation occurs in the ingot, reducing microstructure uniformity and severely impacting the steel's toughness, thus affecting the die's lifespan. Therefore, improving the toughness of hot work die steels is essential to extending die lifespan.

[0004] H11 (4Cr5MoSiV) and H13 (4Cr5MoSiV1) steels possess excellent hot strength, red hardness, high toughness, resistance to thermal fatigue, and resistance to hot cracking. They are air-hardening hot work die steels that combine strength and toughness, and are currently among the most widely used hot work die steels both domestically and internationally. These steels have a high alloy content, making them prone to segregation during electroslag remelting and solidification, resulting in large-sized liquid carbides. To refine these liquid carbides, high-temperature diffusion annealing is typically performed before spheroidizing annealing; however, this process leads to excessively coarse austenite grains. After diffusion annealing, the steel is forged or rolled, but the high forging or rolling temperatures result in still relatively large austenite grain sizes. To further refine the grains, an ultra-fine grain treatment is usually performed before spheroidizing annealing.

[0005] Ultrafine grain refining involves heating a steel ingot above its austenitizing temperature, followed by rapid cooling to generate martensite. Martensite laths are then used to slit the austenite grains, refining the microstructure. However, to suppress excessive austenite grain growth, the ultrafine grain refining temperature is generally controlled at a low level, below 1020℃. Under these conditions, however, a large amount of undissolved carbides remain in the steel, resulting in a final product with numerous large-sized carbides, which is detrimental to improving the strength and toughness of hot work die steel.

[0006] Therefore, improving the toughness of hot work die steel is one of the urgent problems to be solved in this field. Summary of the Invention

[0007] The main objective of this invention is to address the shortcomings of the prior art by providing an ultra-fine heat treatment method for improving the toughness of hot work die steel and a method for preparing high-toughness hot work die steel.

[0008] To achieve the above objectives, the present invention adopts the following technical solution:

[0009] According to a first aspect of the present invention, an ultra-fine heat treatment method for improving the toughness of hot work die steel is provided, comprising the following steps:

[0010] The forged billet is subjected to ultrafine treatment, with a holding temperature of 1020-1080℃ and a holding time of 30-90min;

[0011] The shaped blanks that have undergone ultrafine treatment are tempered at a temperature of 550–600℃ for 1–2 hours.

[0012] The tempered billet is subjected to spheroidizing annealing to obtain finished steel. The spheroidizing annealing temperature is 840-860℃ and the holding time is 1-3h.

[0013] According to one embodiment of the present invention, after the holding time is reached during the spheroidizing annealing process, the formed billet is cooled by a segmented cooling method to obtain the finished steel.

[0014] According to one embodiment of the present invention, the segmented cooling method is as follows: first, the molding blank is cooled to 740°C at a first cooling rate and then kept at that temperature for 4 hours; then, the molding blank is cooled to 500°C at a second cooling rate; then, the molding blank is removed and air-cooled to room temperature, wherein the second cooling rate is greater than the first cooling rate.

[0015] According to one embodiment of the present invention, the first cooling rate is 15-25°C / h, and the second cooling rate is 26-35°C / h.

[0016] According to one embodiment of the present invention, the first cooling rate is 20°C / h, and the second cooling rate is 30°C / h.

[0017] According to one embodiment of the present invention, the size of the forged blank is 500*500*1800mm or more.

[0018] According to a second aspect of the present invention, a method for preparing high-toughness hot work die steel is provided, comprising the following steps:

[0019] The hot work die steel is batched according to its composition content, smelted in an electric furnace, and then electrode rods are cast.

[0020] Electroslag remelting of the electrode rod yields a steel ingot;

[0021] The steel ingot is subjected to diffusion annealing and forging to obtain a steel billet;

[0022] The steel billet is forged to obtain a shaped billet;

[0023] The finished steel product is obtained by subjecting the shaped billet to ultra-fine heat treatment using the method described in the first aspect of the present invention.

[0024] According to one embodiment of the present invention, the composition of the hot work die steel is as follows: by weight percentage, C 0.33-0.43, Si 0.80-1.20, Mn 0.25-0.50, Cr 4.75-5.50, Ni≤0.25, Cu≤0.30, V 0.30-0.60, Mo 1.10-1.60, with the balance being Fe and unavoidable impurities.

[0025] According to one embodiment of the present invention, the diffusion annealing temperature is 1280-1300°C and the holding time is 5-6 hours.

[0026] According to one embodiment of the present invention, the forging heating temperature is 1250-1280°C, and the final forging temperature is greater than 920°C.

[0027] By adopting the above technical solution, the present invention has the following beneficial effects:

[0028] In the present invention, by sequentially subjecting the forged billet to ultrafine treatment, tempering treatment and spheroidizing annealing treatment, and controlling the parameters of each process accordingly, the austenite grain size can be effectively controlled, and carbides can be dispersed and precipitated, which can improve the strength and toughness of hot work die steel, thereby improving the service life of the die. Attached Figure Description

[0029] Figure 1 A flowchart of an ultra-fine heat treatment method for improving the toughness of hot work die steel provided in the first aspect of the present invention.

[0030] Figure 2 A flowchart illustrating a method for preparing high-toughness hot work die steel provided in the second aspect of the present invention.

[0031] Figure 3A and 3B The images shown are scanning electron microscope (SEM) images of the finished steel product and the comparative sample provided in an embodiment of the present invention. Detailed Implementation

[0032] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0033] Specific embodiments of the invention are disclosed herein as needed; however, it should be understood that the embodiments disclosed herein are merely examples of the invention that may be implemented in various alternative forms. In the following description, various operating parameters and components are described in several contemplated embodiments. These specific parameters and components are provided as examples only and are not intended to be limiting.

[0034] As mentioned in the background section, existing hot work die steels contain a large number of large-sized carbides, which is detrimental to improving the strength and toughness of the hot work die steel, and thus affects the service life of the die. To address this technical problem, this invention aims to provide an ultra-fine heat treatment method to improve the toughness of hot work die steel, and a method for preparing high-toughness hot work die steel.

[0035] According to a first aspect of the present invention, an ultra-fine heat treatment method for improving the toughness of hot work die steel is provided, such as... Figure 1 As shown, the ultrafine heat treatment method includes the following steps: S1: ultrafine treatment is performed on the forged billet, with a holding temperature of 1020-1080℃ and a holding time of 30-90 min; S2: the ultrafine treated billet is tempered, with a tempering temperature of 550-600℃ and a tempering time of 1-2 h; S3: the tempered billet is spheroidized annealed to obtain finished steel, with a spheroidizing annealing temperature of 840-860℃ and a holding time of 1-3 h.

[0036] In this invention, by controlling the ultrafine refining temperature between 1020 and 1080°C, the carbides in the steel can be completely dissolved. By performing a low-temperature tempering treatment at 550–600°C, the inheritance of austenite grains can be interrupted, achieving the dual effect of refining austenite grains and promoting the dispersed precipitation of carbides. Therefore, the method of this invention can effectively control the austenite grain size and simultaneously promote the dispersed precipitation of carbides, thereby improving the strength and toughness of hot work die steel and ultimately extending the service life of the die.

[0037] In step S1, the forged billet undergoes an ultra-refining treatment. This involves heating the forged billet above its austenitizing temperature, followed by rapid cooling to generate martensite. Martensite laths are then used to slit the austenite grains, refining the microstructure. In this invention, the holding temperature for the ultra-refining treatment is set to 1020–1080°C, and the holding time is set to 30–90 minutes. This aims to promote complete carbide dissolution, which is beneficial for the dispersed precipitation of carbides during subsequent quenching and tempering heat treatment. If the holding temperature is too low or the holding time is too short, a large amount of carbides may remain undissolved in the steel; if the holding temperature is too high or the holding time is too long, the austenite grain size will be too coarse. Both of these factors are detrimental to improving the strength and toughness of the hot work die steel. During the ultrafine refining process, the holding temperature can typically, but is not limited to, being set to 1020℃, 1030℃, 1040℃, 1050℃, 1060℃, 1070℃, or 1080℃, and the holding time can typically, but is not limited to, being set to 30min, 40min, 50min, 60min, 70min, 80min, or 90min. After the holding time is completed, oil cooling is performed.

[0038] In some embodiments, the size of the forged billet is 500*500*1800mm or larger. As mentioned in the background art, with the increase in the size of hot work die steel, there will be obvious component segregation in the ingot, the uniformity of the microstructure will decrease, and the toughness of the steel will be seriously affected. In other words, it is more difficult to improve the toughness of large-size hot work die steel. The method of the present invention can improve the toughness of large-size hot work die steel (especially hot work die steel with a size of 500*500*1800mm or larger).

[0039] In step S2, the shaped billet after ultra-fine grain treatment is tempered to break the inheritance of austenite grains, achieving the dual effect of refining austenite grains and promoting the dispersed precipitation of carbides. In this invention, the tempering temperature is set to 550-600℃ and the tempering time is set to 1-2 hours to obtain a better comprehensive effect of grain refinement and carbide dispersion precipitation. While maintaining high hardness, strength, and wear resistance, the toughness of the steel is appropriately improved, while significantly reducing the stress and brittleness of the steel. If the tempering temperature is too low or the tempering time is too short, the grain refinement and carbide dispersion precipitation effect will be poor; if the tempering temperature is too high or the tempering time is too long, the grain size will be too coarse, which will be detrimental to improving the strength and toughness of hot work die steel. During the tempering process, the tempering temperature can typically, but not limited to, be set to 550℃, 560℃, 570℃, 580℃, 590℃, or 600℃, and the tempering time can typically, but not limited to, be set to 1h, 1.5h, or 2h.

[0040] In step S3, the spheroidizing annealing treatment is performed on the tempered billet. This refers to heat treatment that causes the layered or network carbides inside the billet to agglomerate into spherical shapes, thereby increasing the toughness of the billet. In this invention, the spheroidizing annealing temperature is controlled at 840–860°C, and the holding time is controlled at 1–3 hours to obtain excellent spheroidized microstructure. During the spheroidizing annealing process, the spheroidizing annealing temperature can typically, but is not limited to, be set to 840°C, 850°C, or 860°C, and the holding time can typically, but is not limited to, be set to 1 hour, 1.5 hours, 2 hours, 2.5 hours, or 3 hours. Preferably, the spheroidizing annealing temperature is 850°C, and the holding time is 2 hours.

[0041] In some embodiments, after the holding time is reached during the spheroidizing annealing process, the formed blank is cooled by a segmented cooling method, which is more conducive to improving the spheroidization effect.

[0042] The segmented cooling method is as follows: first, the formed billet is cooled to 740°C at a first cooling rate, and then held at that temperature for 4 hours; subsequently, the formed billet is cooled to 500°C at a second cooling rate; then, the formed billet is removed and air-cooled to room temperature, wherein the second cooling rate is greater than the first cooling rate. Slow cooling to the two-phase region of 740°C is beneficial for the diffusion of carbon elements in the steel, forming spherical carbides; rapid cooling to below the Al temperature (500°C) is beneficial for saving time and improving production efficiency. Preferably, the first cooling rate is 15–25°C / h, and the second cooling rate is 26–35°C / h. More preferably, the first cooling rate is 20°C / h, and the second cooling rate is 30°C / h.

[0043] According to a second aspect of the present invention, a method for preparing high-toughness hot work die steel is provided, such as... Figure 2 As shown, the preparation method includes the following steps: S10: the raw materials are batched according to the composition content of hot work die steel, smelted in an electric furnace, and electrode rods are cast; S20: the electrode rods are electroslag remelted to obtain steel ingots; S30: the steel ingots are subjected to diffusion annealing and forging to obtain steel billets; S40: the steel billets are forged to obtain shaped billets; S50: the shaped billets are subjected to ultra-fine heat treatment according to the method of the first aspect of the present invention to obtain finished steel products.

[0044] In this invention, the ultra-fine heat treatment method for improving the toughness of hot work die steel, as described in the first aspect of the invention, effectively controls the austenite grain size and allows for the dispersed precipitation of carbides, thereby producing high-toughness hot work die steel. Specifically, in step S20, the electroslag remelting of the electrode rod primarily aims to address quality issues such as segregation and inclusion aggregation during the smelting of large steel ingots, thereby improving the purity of the steel. In step S30, the diffusion annealing and forging of the steel ingot are performed to break dendrites, reduce segregation, and promote primary carbide solution.

[0045] In some embodiments, step S10, batching according to the component content of the hot work die steel, includes batching according to the component content of H11 hot work die steel. The component content of H11 hot work die steel is: by weight percentage, C 0.33-0.43, Si 0.80-1.20, Mn 0.25-0.50, Cr 4.75-5.50, Ni≤0.25, Cu≤0.30, V 0.30-0.60, Mo 1.10-1.60, with the balance being Fe and unavoidable impurities. Although a specific composition of hot work die steel is given herein, it should be understood that the method of the present invention is not limited to this specific composition of hot work die steel, and the method of the present invention is equally applicable to hot work die steels with other compositions, such as H13 hot work die steel.

[0046] In some embodiments, in step S10, smelting in an electric furnace includes smelting in a non-vacuum induction furnace, and casting of electrode rods includes casting electrode rods using a bottom casting method.

[0047] In some embodiments, in step S30, the diffusion annealing temperature is 1280-1300°C, the holding time is 5-6 hours, and the steel ingot is subjected to two upsetting and two drawing processes to break dendrites, reduce segregation, and promote primary carbide solid solution.

[0048] In some embodiments, in step S40, the forging heating temperature is 1250-1280°C, and the final forging temperature is greater than 920°C. Setting the forging heating temperature to 1250-1280°C results in low deformation resistance and uniform microstructure; the final forging temperature greater than 920°C prevents the steel ingot from cracking.

[0049] The present invention will now be described in detail through specific embodiments.

[0050] Example 1

[0051] The 4Cr5MoSiV hot work die steel involved in this invention uses a large steel ingot with dimensions of 500*550*2000mm.

[0052] 1. Non-vacuum induction furnace smelting. The raw materials for this preparation method are mainly recycled materials from Benxi Steel and similar alloy recycled materials, as well as industrial pure iron. The chemical composition of the steel billet, by weight percentage, is: C 0.34, Si 1.0, Mn 0.3, Cr 5.10, Ni 0.2, Cu 0.3, V 0.40, Mo 1.2, with the balance being Fe and unavoidable impurities. Then, the electrode rod is cast using the bottom casting method.

[0053] 2. Electroslag remelting of electrode rods. The main purpose of this invention for electroslag remelting of electrode rods cast in a non-vacuum induction furnace is to solve quality problems such as segregation and inclusion aggregation during the smelting of large steel ingots, thereby improving the purity of the steel.

[0054] 3. The steel ingot is subjected to diffusion annealing and forging. The steel ingot of this invention is a large-sized steel ingot. The diffusion annealing temperature of the steel ingot is 1300℃, the holding time is 5h, and then it is forged.

[0055] 4. Next, the steel billet is forged at a heating temperature of 1250℃ and a final forging temperature of 950℃, resulting in a final ingot size of 500*550*2000mm.

[0056] 5. The formed blank is subjected to ultrafine treatment, and the holding temperature is 1020℃ for 90 minutes to ensure that the carbides are completely dissolved.

[0057] 6. Temper the formed billet at 550℃ for 1 hour to break the inheritance of austenite grains.

[0058] 7. Perform spheroidizing annealing on the sample. The spheroidizing temperature is 850℃ and held for 2 hours. Then, the temperature is reduced to 740℃ at a rate of 20℃ / h and held for 4 hours. After that, the temperature is reduced to 500℃ at a rate of 30℃ / h and then air-cooled to obtain the finished annealed steel.

[0059] 8. The sample was oil-quenched at 1000℃ for 30 minutes, followed by tempering at 590℃ for 2 hours and then tempering at 600℃ for 2 hours, resulting in a shape of 10*10*55mm. The V-notch impact energy was 23J, representing a 30% improvement in toughness compared to the control sample. The difference between the control sample and Example 1 lies in the ultrafine grinding and tempering processes. The control sample process was as follows: Step 5 involved ultrafine grinding of the formed blank at 970℃ for 45 minutes, followed by oil cooling. Step 6, tempering, was omitted; subsequent steps were the same as in Example 1.

[0060] The sample obtained in Example 1 and the control sample were characterized by scanning electron microscopy, and the results are as follows: Figure 3A and 3B As shown, where, Figure 3A Corresponding to the sample in Example 1, Figure 3BCorresponding to the control sample. As can be seen from the figure: in the sample of Example 1, the carbide size is smaller and it precipitates in a diffuse manner, while in the control sample, the carbide size is relatively larger and the dispersion is not uniform.

[0061] Example 2

[0062] The 4Cr5MoSiV hot work die steel involved in this invention uses a large steel ingot with dimensions of 600*550*1800mm.

[0063] 1. Non-vacuum induction furnace smelting. The raw materials for this preparation method are mainly recycled materials from Benxi Steel and similar alloy recycled materials, as well as industrial pure iron. The chemical composition of the steel billet, by weight percentage, is: C 0.35, Si 1.2, Mn 0.4, Cr 5.21, Ni 0.18, Cu 0.25, V 0.38, Mo 1.3, with the balance being Fe and unavoidable impurities. The electrode rod is then cast using the bottom casting method.

[0064] 2. Electroslag remelting of the electrode rod.

[0065] 3. The steel ingot is subjected to diffusion annealing and forging. The steel ingot of this invention is a large-sized steel ingot. The diffusion annealing temperature of the steel ingot of this invention is 1300℃, and the holding time is 5h, followed by forging.

[0066] 4. Next, the steel billet is forged at a heating temperature of 1250℃ and a final forging temperature of 950℃, resulting in a final ingot size of 600*550*1800mm.

[0067] 5. The formed blank is subjected to ultrafine treatment, and the holding temperature is 1050℃ for 45 minutes to ensure that the carbides are completely dissolved.

[0068] 6. Temper the formed billet at 550℃ for 1 hour to break the inheritance of austenite grains.

[0069] 7. Perform spheroidizing annealing on the sample. The spheroidizing temperature is 850℃ and held for 2 hours. Then, the temperature is reduced to 740℃ at a rate of 20℃ / h and held for 4 hours. After that, the temperature is reduced to 500℃ at a rate of 30℃ / h and then air-cooled to obtain the finished annealed steel.

[0070] 8. The sample was oil-quenched at 1000℃ for 30 minutes, followed by tempering at 590℃ for 2 hours and then tempering at 600℃ for 2 hours, resulting in a shape of 10*10*55mm. The V-notch impact energy was 24J, representing a 33% improvement in toughness compared to the control sample. The difference between the control sample and Example 2 lies in the ultrafine grinding and tempering processes. The control sample process was as follows: Step 5 involved ultrafine grinding of the formed blank at 970℃ for 45 minutes, followed by oil cooling. Step 6, tempering, was omitted; subsequent steps were the same as in Example 2.

[0071] Example 3

[0072] The 4Cr5MoSiV hot work die steel involved in this invention uses a large steel ingot with dimensions of 600*580*1800mm.

[0073] 1. Non-vacuum induction furnace smelting. The raw materials for this preparation method are mainly recycled materials from Benxi Steel and similar alloy recycled materials, as well as industrial pure iron. The chemical composition of the steel billet, by weight percentage, is: C 0.35, Si 1.2, Mn 0.4, Cr 5.21, Ni 0.18, Cu 0.25, V 0.38, Mo 1.3, with the balance being Fe and unavoidable impurities. The electrode rod is then cast using the bottom casting method.

[0074] 2. Electroslag remelting of the electrode rod.

[0075] 3. The steel ingot is subjected to diffusion annealing and forging. The steel ingot of this invention is a large-sized steel ingot. The diffusion annealing temperature of the steel ingot of this invention is 1300℃, and the holding time is 5h, followed by forging.

[0076] 4. Next, the steel billet is forged at a heating temperature of 1250℃ and a final forging temperature of 950℃, resulting in a final ingot size of 600*580*1800mm.

[0077] 5. The formed blank is subjected to ultrafine treatment, and the holding temperature is 1050℃ for 45 minutes to ensure that the carbides are completely dissolved.

[0078] 6. Temper the formed billet at 580℃ for 1 hour to break the inheritance of austenite grains.

[0079] 7. Perform spheroidizing annealing on the sample. The spheroidizing temperature is 850℃ and held for 2 hours. Then, the temperature is reduced to 740℃ at a rate of 20℃ / h and held for 4 hours. After that, the temperature is reduced to 500℃ at a rate of 30℃ / h and then air-cooled to obtain the finished annealed steel.

[0080] 8. The sample was oil-quenched at 1000℃ for 30 minutes, followed by tempering at 590℃ for 2 hours and then tempering at 600℃ for 2 hours, resulting in a shape of 10*10*55mm. The V-notch impact energy was 22J, representing a 22% improvement in toughness compared to the control sample. The difference between the control sample and Example 3 lies in the ultrafine grinding and tempering processes. The control sample process was as follows: Step 5, the formed blank was ultrafine ground at 970℃ for 45 minutes, followed by oil cooling. Step 6, the tempering process, was omitted; subsequent steps were the same as in Example 3.

[0081] Example 4

[0082] The 4Cr5MoSiV hot work die steel involved in this invention uses a large steel ingot with dimensions of 600*580*1800mm.

[0083] 1. Non-vacuum induction furnace smelting. The raw materials for this preparation method are mainly recycled materials from Benxi Steel and similar alloy recycled materials, as well as industrial pure iron. The chemical composition of the steel billet, by weight percentage, is: C 0.35, Si 1.2, Mn 0.4, Cr 5.21, Ni 0.18, Cu 0.25, V 0.38, Mo 1.3, with the balance being Fe and unavoidable impurities. The electrode rod is then cast using the bottom casting method.

[0084] 2. Electroslag remelting of the electrode rod.

[0085] 3. The steel ingot is subjected to diffusion annealing and forging. The steel ingot of this invention is a large-sized steel ingot. The diffusion annealing temperature of the steel ingot of this invention is 1280℃, and the holding time is 6h, followed by forging.

[0086] 4. Next, the steel billet is forged at a heating temperature of 1280℃ and a final forging temperature of 950℃, resulting in a final ingot size of 600*580*1800mm.

[0087] 5. The formed blank is subjected to ultrafine treatment, and the holding temperature is 1080℃ for 30 minutes to ensure that the carbides are completely dissolved.

[0088] 6. Temper the formed billet at 600℃ for 2 hours to break the inheritance of austenite grains.

[0089] 7. Perform spheroidizing annealing on the sample. The spheroidizing temperature is 850℃ and held for 2 hours. Then, the temperature is reduced to 740℃ at a rate of 20℃ / h and held for 4 hours. After that, the temperature is reduced to 500℃ at a rate of 30℃ / h and then air-cooled to obtain the finished annealed steel.

[0090] 8. The sample was oil-quenched at 1000℃ for 30 minutes, followed by tempering at 590℃ for 2 hours and then tempering at 600℃ for 2 hours, resulting in a shape of 10*10*55mm. The V-notch impact energy was 22J, representing a 25% improvement in toughness compared to the control sample. The difference between the control sample and Example 4 lies in the ultrafine grinding and tempering processes. The control sample process was as follows: Step 5, the formed blank was ultrafine ground at 970℃ for 45 minutes, followed by oil cooling. Step 6, the tempering process, was omitted; subsequent steps were the same as in Example 4.

[0091] Finally, it should be noted that the embodiments described above are only some, not all, of the embodiments of the present invention. The detailed description of the embodiments of the present invention is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

Claims

1. A method for ultra-fine heat treatment to improve the toughness of hot work die steel, characterized in that, Includes the following steps: The forged billet is subjected to ultra-fine refining treatment at a holding temperature of 1020–1080℃ for 30–90 minutes, resulting in a forged billet size of 500 mm. 500 1800 mm or more; The shaped blanks that have undergone ultrafine treatment are tempered at a temperature of 550-600℃ for 1-2 hours. The tempered billet is then subjected to spheroidizing annealing to obtain finished steel. The spheroidizing annealing temperature is 840~860℃, and the holding time is 1~3h. During the spheroidizing annealing process, after the holding time is reached, the formed billet is cooled using a segmented cooling method to obtain the finished steel product. The segmented cooling method is as follows: first, the molded blank is cooled to 740°C at the first cooling rate and then kept at that temperature for 4 hours; then, the molded blank is cooled to 500°C at the second cooling rate; after that, the molded blank is taken out and air-cooled to room temperature, wherein the second cooling rate is greater than the first cooling rate.

2. The ultra-fine heat treatment method for improving the toughness of hot work die steel according to claim 1, characterized in that, The first cooling rate is 15~25℃ / h, and the second cooling rate is 26~35℃ / h.

3. The ultra-fine heat treatment method for improving the toughness of hot work die steel according to claim 2, characterized in that, The first cooling rate is 20℃ / h, and the second cooling rate is 30℃ / h.

4. A method for preparing high-toughness hot work die steel, characterized in that, Includes the following steps: The hot work die steel is batched according to its composition content, smelted in an electric furnace, and then electrode rods are cast. Electroslag remelting of the electrode rod yields a steel ingot; The steel ingot is subjected to diffusion annealing and forging to obtain a steel billet; The steel billet is forged to obtain a shaped billet; The shaped billet is subjected to ultra-fine heat treatment according to any one of claims 1-3 to obtain finished steel products.

5. The method for preparing high-toughness hot work die steel according to claim 4, characterized in that, The composition of hot work die steel is as follows (by weight percentage): C 0.33–0.43, Si 0.80–1.20, Mn 0.25–0.50, Cr 4.75–5.50, Ni ≤0.25, Cu ≤0.30, V 0.30–0.60, Mo 1.10–1.60, with the balance being Fe and unavoidable impurities.

6. The method for preparing high-toughness hot work die steel according to claim 4, characterized in that, The diffusion annealing temperature is 1280~1300℃, and the holding time is 5~6h.

7. The method for preparing high-toughness hot work die steel according to claim 4, characterized in that, The forging heating temperature is 1250~1280℃, and the final forging temperature is greater than 920℃.

Citation Information

Patent Citations

  • Annealing heat treatment method of H13 die steel

    CN103333997A

  • Manufacturing method of high-performance hot work die steel

    CN113621876A