A method for recovering valuable metals from zinc calcine by using aluminum ash residue for synergistic treatment
By calcining aluminum ash slag with zinc calcined sand, zinc ferrite is decomposed into gaseous zinc and aluminum nitride is converted into aluminum oxide, which solves the problems of difficult zinc ferrite recovery and the danger of aluminum ash slag treatment, and realizes efficient recovery of valuable metals.
Patent Information
- Application Number
- CN202410016278.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-05
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-01-05
AI Technical Summary
Existing technologies are insufficient for the efficient recovery of valuable metals from zinc ferrite and aluminum ash slag. In particular, the instability of zinc ferrite leads to zinc loss, and the treatment of aluminum ash slag is dangerous and wasteful of resources.
Aluminum ash slag is mixed with zinc calcined sand and roasted under an inert atmosphere. By controlling a certain ratio and temperature, zinc ferrite is decomposed into gaseous zinc dust through the roasting reaction, and aluminum nitride is converted into aluminum oxide, thus realizing the separation and recovery of valuable metals.
It achieves a high recovery rate of zinc ferrite (over 90%), reduces the danger of aluminum ash slag, simplifies the processing flow, and improves metal recovery and resource utilization.
Smart Images

Figure BDA0004650927240000041 
Figure BDA0004650927240000042 
Figure BDA0004650927240000051
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid waste treatment technology, and specifically to a method for recovering valuable metals from zinc calcined sand by co-processing aluminum ash slag. Background Technology
[0002] Zinc ferrite is a byproduct of traditional hydrometallurgical zinc recovery processes. In zinc production, 85% of the output comes from hydrometallurgical zinc refining, resulting in a large amount of difficult-to-recover zinc slag. Furthermore, mining is subject to certain restrictions due to policy influences, making the recovery of this waste slag essential. Zinc ferrite is one of the most difficult substances to react with and recover during zinc recovery due to its stable spinel structure, making it poorly soluble in acids. Zinc ferrite's chemical stability causes zinc loss during conventional recovery processes, making its recovery a critical aspect of zinc recovery.
[0003] Aluminum slag is a byproduct of aluminum electrolysis. As of 2021, 15-20 tons of aluminum slag were generated for every ton of aluminum electrolyzed. Based on chemical composition and formation process, it can be divided into primary aluminum slag and secondary aluminum slag. Primary aluminum slag mainly consists of alumina formed when aluminum comes into contact with air during electrolysis. Secondary aluminum slag is a black residue generated during the recycling of primary aluminum slag and waste aluminum. Secondary aluminum slag, also known as aluminum ash, mainly contains aluminum nitride, alumina, aluminum carbide, spinel, and other components. 80% of primary aluminum slag is converted into secondary aluminum slag after recycling. Therefore, secondary aluminum slag is the main waste generated during aluminum electrolysis. Due to the gap between aluminum demand and production, the recycling of aluminum ash is feasible. However, due to the highly reactive nature of aluminum nitride in aluminum ash, the recycling process of secondary aluminum slag carries certain risks. Current research on aluminum ash mainly focuses on using aluminum nitride in aluminum ash as a reducing agent to reduce heavy metals in sludge, or using aluminum-rich components as raw materials for ceramic synthesis.
[0004] Currently, many researchers have conducted research on the reduction of nitrogen chloride in aluminum ash slag and the recovery of zinc ferrite. For example, CN202211392154.0 discloses a method for preparing aluminum-silicon alloys from aluminum ash slag. The aluminum ash slag is crushed and added to an electrolytic cell along with a certain amount of silica sand and alumina. Using molten salt electrolysis, an aluminum-silicon alloy with a suitable silicon content can be produced, achieving precise recovery of silicon and aluminum elements from the aluminum ash slag with minimal oxidation loss and a high recovery rate. However, this patent does not address the classification and application of various aluminum-containing compounds in the aluminum ash slag, resulting in some waste. CN201910329092.0 discloses a method for recovering and reusing aluminum ash slag. After crushing the aluminum ash slag, iron impurities are first separated by magnetic separation, and metallic aluminum is separated by screening. Then, aluminum nitride and salts are decomposed by water washing to obtain alumina filter residue. The aluminum residue is then wet-milled with additives such as kaolin, bentonite, and talc to form a slurry, which is then fired to obtain foam ceramics. This effectively improves the utilization rate of aluminum ash slag and reduces environmental pollution. However, this patent simply converts aluminum nitride into aluminum oxide with water without utilizing the reaction characteristics of aluminum nitride. Therefore, further research is needed on the characteristics of aluminum ash slag. CN201410735389.4 discloses a method for enhancing the selective decomposition of zinc ferrite. First, pyrochemical reduction roasting is performed at high temperature, followed by magnetized roasting after a certain temperature reduction. After cooling, iron and zinc are separated and recovered using acid leaching and magnetic separation. This method improves the decomposition rate of zinc ferrite and the magnetization effect of the iron phase. However, the acid leaching process generates waste liquid, causing environmental pollution. Further research is needed on pollution-free recovery of zinc ferrite. Summary of the Invention
[0005] The purpose of this invention is to at least solve one of the technical problems existing in the prior art, and to provide a method for recovering valuable metals by co-processing zinc calcined sand with aluminum ash slag.
[0006] The technical solution of the present invention is as follows:
[0007] A method for recovering valuable metals from zinc calcined sand by co-processing aluminum ash slag involves mixing aluminum ash slag containing aluminum nitride with zinc calcined sand containing zinc ferrite, ball milling the mixture, and calcining it under an inert atmosphere. The zinc-containing components in the zinc calcined sand decompose and release zinc fumes, which are then collected.
[0008] Furthermore, the mass ratio of the aluminum ash powder to zinc ferrite is controlled at 1:1 to 7.
[0009] Furthermore, the aluminum ash contains >20 wt% aluminum nitride.
[0010] Furthermore, the zinc calcinate contains >50 wt% zinc ferrite.
[0011] Furthermore, it includes the following steps:
[0012] S1: Crush and dry aluminum ash slag and zinc calcined sand separately, and pulverize them to a particle size of 80-200 mesh to obtain aluminum ash slag powder and zinc calcined sand powder.
[0013] S2: Mix aluminum ash powder and zinc calcined sand powder evenly, place them in an inert protective atmosphere for roasting, and collect the smoke and dust generated during roasting.
[0014] Further, in step S2, the calcination includes: heating to a target temperature and maintaining the temperature for a period of time, wherein the target temperature is 900 to 1400°C and the temperature is maintained at the target temperature for 0.5 to 1.5 hours.
[0015] Furthermore, in step S2, the heating rate is 5–10 °C / min.
[0016] Furthermore, in step S1, the drying temperature is 90-110℃, and the drying time is 2-4 days.
[0017] This invention has at least one of the following beneficial effects:
[0018] (1) The present invention provides a method for recovering valuable metals by co-processing zinc calcined sand with aluminum ash slag. Through the mutual reaction between aluminum ash slag and zinc ferrite, the difficult-to-recover zinc ferrite is separated from the reactants in gaseous form, which solves the problem of difficult recovery of zinc ferrite and ensures that the zinc recovery rate reaches more than 90%.
[0019] (2) The present invention provides a method for co-processing zinc calcined sand to recover valuable metals using aluminum ash slag. By adding aluminum ash slag, the aluminum nitride portion of which reacts with zinc ferrite and converts it into alumina, which is far less dangerous than aluminum nitride, thereby reducing the danger of aluminum ash slag during transportation, storage and recycling.
[0020] (3) The present invention provides a method for recovering valuable metals by co-processing zinc roasted sand with aluminum ash slag. The method adopts an integrated process to separate zinc from the solid and convert aluminum nitride into aluminum oxide, thereby reducing the impurities contained in aluminum ash slag, recovering zinc, and is simple to operate with a high metal recovery rate. It also reduces a large number of subsequent processes for separating and purifying metals, and reduces the excess impurities and recovery difficulties of aluminum ash slag during recovery. Attached Figure Description
[0021] Figure 1 This is a schematic flowchart of a method for recovering valuable metals from zinc calcined sand using aluminum ash slag co-processing according to the present invention.
[0022] Figure 2 Here is an SEM image of the smoke and dust collected in Example 1;
[0023] Figure 3 EDS image of the collected smoke dust in Example 1. Detailed Implementation
[0024] The embodiments of the present invention are described in detail below. These embodiments are exemplary and are only used to explain the present invention, and should not be construed as limiting the invention. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in the art or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all commercially available conventional products.
[0025] It should be noted that the aluminum ash and zinc calcined sand in the examples were both sourced from Shanghai Maclean Biochemical Technology Co., Ltd., China. The aluminum ash was crushed and dried in an oven at 100±5℃ for 3 days. The dried aluminum ash was then mixed and pulverized in a pulverizer to achieve a particle size of 80–200 mesh. The specific types and contents of compounds in the aluminum ash and zinc calcined sand are shown in Tables 1 and 2.
[0026] Table 1. Types and contents of various compounds in aluminum ash slag
[0027]
[0028] Table 2. Types and contents of various compounds in zinc roasting slag.
[0029]
[0030]
[0031] Example 1
[0032] like Figure 1 As shown, a method for recovering valuable metals from zinc calcined abrasive using aluminum ash slag co-processing is described. The specific steps are as follows: 6.4g of dried and pulverized 150-mesh zinc calcined abrasive powder and 1.6g of dried and pulverized 150-mesh aluminum ash slag powder are mixed evenly and placed in a tube furnace. After evacuation, argon gas is introduced. A calcination experiment is conducted on the mixed powder at a flow rate of 100ml / min, with a heating rate of 10℃ / min, a target temperature of 1300℃, and a calcination duration of 1h. The smoke and dust generated during the entire experiment are collected.
[0033] Example 2
[0034] like Figure 1 As shown, a method for recovering valuable metals from zinc calcined abrasive using aluminum ash slag co-processing is described. The specific steps are as follows: 6.4g of dried and pulverized 150-mesh zinc calcined abrasive powder and 1.6g of dried and pulverized 150-mesh aluminum ash slag powder are mixed evenly and placed in a tube furnace. After evacuation, argon gas is introduced. A calcination experiment is conducted on the mixed powder at a flow rate of 100ml / min, with a heating rate of 10℃ / min, a target temperature of 1200℃, and a calcination duration of 1h. The smoke and dust generated during the entire experiment are collected.
[0035] Example 3
[0036] like Figure 1 As shown, a method for recovering valuable metals from zinc calcined abrasive using aluminum ash slag co-processing is described. The specific steps are as follows: 6.4g of dried and pulverized 150-mesh zinc calcined abrasive powder and 1.6g of dried and pulverized 150-mesh aluminum ash slag powder are mixed evenly and placed in a tube furnace. After evacuation, argon gas is introduced. A calcination experiment is conducted on the mixed powder at a flow rate of 100ml / min, with a heating rate of 10℃ / min, a target temperature of 1000℃, and a calcination duration of 1h. The smoke and dust generated during the entire experiment are collected.
[0037] Example 4
[0038] like Figure 1 As shown, a method for recovering valuable metals from zinc calcined abrasive using aluminum ash slag co-processing is described. The specific steps are as follows: 6.4g of dried and pulverized 150-mesh zinc calcined abrasive powder and 1.6g of dried and pulverized 150-mesh aluminum ash slag powder are mixed evenly and placed in a tube furnace. After evacuation, argon gas is introduced. A calcination experiment is conducted on the mixed powder at a flow rate of 100ml / min, with a heating rate of 10℃ / min, a target temperature of 1300℃, and a calcination duration of 0.5h. The smoke and dust generated during the entire experiment are collected.
[0039] Example 5
[0040] like Figure 1 As shown, a method for recovering valuable metals from zinc calcined abrasive using aluminum ash slag co-processing is described. The specific steps are as follows: 6.4g of dried and pulverized 150-mesh zinc calcined abrasive powder and 0.8g of dried and pulverized 150-mesh aluminum ash slag powder are mixed evenly and placed in a tube furnace. After evacuation, argon gas is introduced. A calcination experiment is conducted on the mixed powder at a flow rate of 100ml / min, with a heating rate of 10℃ / min, a target temperature of 1300℃, and a calcination duration of 1h. The smoke and dust generated during the entire experiment are collected.
[0041] Comparative Example 1 (Single Powder Calcination)
[0042] One of the two mixed powders was selected to conduct a method for recovering valuable metals from zinc calcined sand by co-processing with aluminum ash slag. The specific experimental steps were as follows: 6.4g of dried and pulverized 150-mesh zinc calcined sand powder was placed in a tube furnace, and after evacuation, argon gas was introduced at a flow rate of 100ml / min. The calcination temperature was 1200℃ and the calcination time was 1h. The volatile dust was collected.
[0043] Comparative Example 2 (Single Powder Calcination)
[0044] A comparative experiment was conducted on one of the two mixed powders, using aluminum ash slag to co-process zinc calcined sand to recover valuable metals. The specific experimental steps were as follows: 1.6g of dried and pulverized 150-mesh aluminum ash slag powder was placed in a tube furnace, vacuumed, and argon gas was introduced at a flow rate of 100ml / min. The calcination temperature was 1200℃, the calcination time was 1h, and the volatile dust was collected.
[0045] After the above examples and comparative examples were roasted, the roasted residue was cooled to room temperature, removed, and ground. A small portion of the roasted residue and flue dust was taken out to determine the metal types and contents. The zinc recovery rate and aluminum nitride residue rate of each example were measured and calculated, as shown in the table below:
[0046] Table 3 Summary of Zinc Recovery and Aluminum Nitride Residual Rate After Calcination in Examples and Comparative Examples
[0047]
[0048] As shown in Table 2, zinc and aluminum were separated in the examples. The main metal in the flue dust was zinc, and the main metal in the roasting slag was aluminum. The zinc recovery rate exceeded 90%, reaching 96.4%. Over 90% of the aluminum nitride in the aluminum ash slag was converted to alumina. Example 1 was the optimal method, with a 20% aluminum ash slag addition, appropriate temperature, and roasting time all contributing to an overall improvement in the recovery rate of zinc and the conversion of aluminum nitride. The experimental results from the examples and comparative examples show that using aluminum ash slag to co-process zinc roasting sand for valuable metal recovery can effectively extract zinc from zinc ferrite and reduce the reactivity of aluminum ash slag. This is a practical method for the resource utilization of valuable metals from metallurgical slag. Further research and advancement are warranted because during the roasting experiment, the conversion of aluminum nitride to alumina generates a large amount of nitrogen and heat, sublimating the reacted elemental zinc or zinc oxide into a gaseous state. The nitrogen generated during the reaction separates from the mixture, allowing zinc to separate as well, and converting aluminum nitride into the less hazardous alumina. SEM-EDS analysis of the flue dust collected in Example 1 yielded the following results: Figure 2 and Figure 3 As shown in the figure, a small amount of aluminum oxide and aluminum nitride powder was detected in the smoke. This may be because nitrogen gas was separated from the solid during the experiment.
[0049] The embodiments described above are merely preferred embodiments of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various other corresponding changes and modifications based on the technical solutions and concepts described above, and all such changes and modifications should fall within the protection scope of the claims of the present invention.
Claims
1. A method for recovering valuable metals from zinc roasted sand by co-processing aluminum ash slag, characterized in that, Aluminum ash containing aluminum nitride is mixed with zinc calcined sand containing zinc ferrite and ball-milled. The mixture is then roasted under an inert atmosphere. The zinc-containing components in the zinc calcined sand decompose and release zinc fumes. The fumes generated during the reaction are collected. The mass ratio of aluminum ash powder to zinc ferrite is controlled at 1:1 to 7. The aluminum ash contains >20wt% aluminum nitride; The zinc calcinate contains >50wt% zinc ferrite; The roasting process includes: heating to a target temperature and maintaining the temperature for a period of time, wherein the target temperature is 900 to 1400°C and the temperature is maintained at the target temperature for 0.5 to 1.5 hours.
2. The method for recovering valuable metals from zinc roasted sand using aluminum ash slag co-processing according to claim 1, characterized in that, Includes the following steps: S1: Crush and dry aluminum ash slag and zinc calcined sand separately, and pulverize them to a particle size of 80-200 mesh to obtain aluminum ash slag powder and zinc calcined sand powder. S2: Mix aluminum ash powder and zinc calcined sand powder evenly, place them in an inert protective atmosphere for roasting, and collect the smoke and dust generated during roasting.
3. The method for recovering valuable metals from zinc roasted sand using aluminum ash slag co-processing according to claim 2, characterized in that, In step S2, the heating rate is 5–10 °C / min.
4. The method for recovering valuable metals from zinc roasted sand by co-processing with aluminum ash slag according to claim 2, characterized in that, In step S1, the drying temperature is 90-110℃, and the drying time is 2-4 days.
Citation Information
Patent Citations
A method for strengthening the selective decomposition of zinc ferrite
CN104451126B
Aluminum ash recovering and reutilizing method
CN109970456A
Method for preparing aluminum-silicon alloy by recycling aluminum ash
CN115652370A
Method for recovering metal resource from zinc calcine through reduction roasting-leaching-zinc sinking
CN104946903A
Harmless dressing and smelting method for recycling lead, zinc, carbon, iron and tailings from water quenching slag
CN109825718A