A positive electrode sheet, a method for manufacturing the same, a secondary battery, and an electric device
By setting a flame-retardant layer with a specific compaction density between the positive electrode current collector and the positive electrode material layer, and controlling the particle size relationship between the flame-retardant and conductive materials, the negative impact of flame-retardant additives on battery transmission is solved, thereby improving the electrochemical performance and energy density of the battery.
Patent Information
- Application Number
- CN202410150953.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-02
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-02-02
AI Technical Summary
While existing technologies aim to improve battery safety, flame retardant additives can affect ion transport in the electrolyte and the stability of the electrochemical reaction interface, as well as increase the internal resistance of the cell and reduce battery efficiency.
A flame-retardant layer with a specific compaction density is set between the positive electrode current collector and the positive electrode material layer. This layer contains flame-retardant materials, conductive materials, and a binder. The relationship between the primary particle size D50 of the flame-retardant materials and conductive materials in the flame-retardant layer is controlled to ensure that the flame-retardant materials are introduced in solid form without affecting the transport of electrolyte and positive electrode active material ions.
It improves the electrochemical performance of the battery, ensures the stability of the electrochemical reaction interface, enhances electron transport capability, improves the battery's energy density and internal resistance, and avoids interference from flame-retardant materials on the transport of electrolyte and positive electrode active materials.
Smart Images

Figure CN117976814B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of new energy technology, specifically to a positive electrode sheet and its preparation method, a secondary battery and electrical equipment. Background Technology
[0002] Safety has always been a critical concern in the battery industry. Currently, the main approach is to add appropriate flame-retardant additives, such as phosphate esters, phosphites, organohalogenated compounds, or phosphazenes, to the electrolyte to improve battery safety. However, these flame-retardant additives can affect ion transport in the electrolyte, reduce the stability of the electrochemical reaction interface, and impact the overall cycle life of the battery. There are also reports of using a flame-retardant layer between the positive electrode and the separator to improve battery safety. However, this not only increases the ion diffusion distance of the positive electrode active material, increasing the cell's internal resistance and reducing cell efficiency, thus hindering performance, but the flame-retardant layer also lacks ion transport capabilities, significantly reducing ion diffusion-transport capacity within the electrolyte phase, lowering the battery's rate cycle energy, reducing battery efficiency, and impairing its electrochemical performance. Therefore, it is necessary to develop a technology that can improve battery safety without affecting ion transport in the electrolyte, interfering with the stability of the electrochemical reaction interface, or interfering with the ion transport of the positive electrode active material. Summary of the Invention
[0003] Based on the deficiencies of the existing technology, the purpose of this application is to provide a positive electrode sheet and its preparation method, a secondary battery and an electrical device.
[0004] To achieve the above objectives, in a first aspect, this application provides a positive electrode sheet, including a current collector, wherein a flame-retardant layer is provided on at least one side of the current collector, and a positive electrode material layer is provided on the surface of the flame-retardant layer opposite to the current collector.
[0005] The flame-retardant layer comprises a flame-retardant material, a conductive material, and an adhesive, and satisfies the following relationship:
[0006] 1 / 2D1 <D2<D1,
[0007] Wherein, D1 is the primary particle size D50 of the conductive material in the flame-retardant layer.
[0008] D2 is the primary particle size D50 of the flame-retardant material in the flame-retardant layer;
[0009] The compacted density of the flame-retardant layer is 0.19-2.1 g / cm³. 3 .
[0010] Preferably, D2 / D1 = 0.75.
[0011] Preferably, D1 = 90-4100nm, D2 = 40-3100nm.
[0012] Preferably, the areal density of the flame-retardant layer is 3.9-21 g / cm³. 2 .
[0013] Preferably, at least one of features a)-c) is also satisfied:
[0014] a) The flame-retardant material in the flame-retardant layer includes at least one of antimony trioxide, brominated polystyrene, aluminum hydroxide, magnesium hydroxide, and ammonium polyphosphate;
[0015] b) The conductive material in the flame-retardant layer includes at least one of carbon nanotubes, graphene, and conductive carbon black;
[0016] c) The binder in the flame-retardant layer includes at least one of polyethylene oxide, polytetrafluoroethylene, polyacrylic acid, sodium hydroxymethyl cellulose, and styrene-butadiene rubber.
[0017] Secondly, this application provides a method for preparing the positive electrode sheet, comprising the following steps:
[0018] Flame-retardant materials, conductive materials, and binders are dispersed in a solvent to obtain a flame-retardant slurry;
[0019] The flame-retardant slurry is coated onto at least one side of the current collector, rolled, and then dried to form a flame-retardant layer.
[0020] A positive electrode material slurry is coated on the surface of the flame-retardant layer facing away from the current collector, and then a second drying process is performed to obtain a positive electrode sheet.
[0021] Thirdly, this application provides a secondary battery, including the positive electrode sheet or the positive electrode sheet prepared by the preparation method.
[0022] Fourthly, this application provides an electrical device including the aforementioned secondary battery.
[0023] Compared to existing technologies, the advantages of this application are as follows: By setting a flame-retardant layer with a specific compaction density between the positive electrode current collector and the positive electrode material layer, the flame-retardant material is introduced in a solid form, ensuring that the introduction of the flame-retardant material does not affect the transport of ions in the electrolyte, thus making the electrochemical reaction interface more stable; it also ensures that there are no obstacles between the positive electrode material layer and the separator, so as not to interfere with the transport of ions in the positive electrode active material or the transport of ions in the electrolyte. At the same time, this application improves the electron transport capability of the flame-retardant layer by controlling the primary particle size D50 of the flame-retardant material and the conductive material in the flame-retardant layer to meet a specific relationship, thereby improving the electrochemical performance of the battery. Attached Figure Description
[0024] Figure 1This is a schematic diagram of the structure of the positive electrode sheet in one embodiment of this application, wherein 1 is aluminum foil, 2 is flame retardant material, 3 is conductive material, and 4 is positive electrode material layer;
[0025] Figure 2 The process flow diagram for preparing the positive electrode sheet in Example 1 is shown. Detailed Implementation
[0026] To better illustrate the purpose, technical solutions, and advantages of this application, the following description, in conjunction with specific embodiments and comparative examples, aims to provide a detailed understanding of the content of this application, rather than limiting it. All other embodiments obtained by those skilled in the art without inventive effort are within the protection scope of this application. Unless otherwise specified, the experimental reagents and instruments involved in the implementation of this application are commonly used reagents and instruments. In this application, the technical features described in an open-ended manner include both closed-ended technical solutions composed of the listed features and open-ended technical solutions that include the listed features.
[0027] According to a first aspect of this application, a positive electrode sheet is provided, which includes a current collector, a flame retardant layer is provided on at least one side of the current collector, and a positive electrode material layer is provided on the surface of the flame retardant layer facing away from the current collector.
[0028] The aforementioned flame-retardant layer comprises flame-retardant material, conductive material, and adhesive, and satisfies the following relationship:
[0029] 1 / 2D1 <D2<D1,
[0030] Wherein, D1 is the primary particle size D50 of the conductive material in the aforementioned flame-retardant layer.
[0031] D2 is the primary particle size D50 of the flame-retardant material in the flame-retardant layer mentioned above;
[0032] The compacted density of the flame-retardant layer is 0.19-2.1 g / cm³. 3 .
[0033] This application solves the problem of negative effects of adding flame retardant additives to the battery by setting a flame retardant layer with a specific compaction density between the positive electrode current collector and the positive electrode material layer, allowing the flame retardant material to be introduced in solid form. This ensures that the introduction of the flame retardant material does not affect the transport of ions in the electrolyte, making the electrochemical reaction interface more stable; it also ensures that there are no obstacles between the positive electrode material layer and the separator, so as not to interfere with the transport of positive electrode active material ions and the transport of ions in the electrolyte.
[0034] The compaction density of the flame-retardant layer needs to be controlled between 0.19 and 2.1 g / cm³. 3Within this range, on the one hand, the flame-retardant layer has lower porosity, resulting in a larger contact area between the flame-retardant material and the conductive material, and stronger electron transport capability. On the other hand, reducing the thickness of the inactive components can significantly improve the overall energy density of the battery cell. If the compaction density of the flame-retardant layer is less than 0.19 g / cm³, the overall energy density of the battery cell can be significantly improved. 3 The flame-retardant layer will become significantly thicker, reducing the energy density of the battery cell. If the compaction density of the flame-retardant layer is greater than 2.1 g / cm³... 3 It has poor flame retardant properties.
[0035] In addition, this application improves the electron transport capability of the flame-retardant layer by controlling the primary particle size D50 of the flame-retardant material and the conductive material in the flame-retardant layer to satisfy the above relationship, thereby enhancing the performance of the battery's electrochemical properties and improving the flame-retardant effect.
[0036] Optionally, D2 / D1 can be 0.6, 0.75, 0.9, etc. Preferably, D2 / D1 is 0.75.
[0037] Preferably, D1 = 90-4100nm. When D1 < 90nm, the particle size of the conductive material is too small, making it difficult to form a continuous conductive network and reducing the conductivity. When D1 > 4100nm, the particle size of the conductive particles is too large, resulting in an excessively thick flame-retardant layer and reducing the energy density of the positive electrode.
[0038] Preferably, D2 = 40-3100nm. When D2 < 40nm, the particle size of the flame retardant material is too small, and it is easy to agglomerate during the dispersion process, which reduces the flame retardant effect; when D2 > 3100nm, the particle size of the flame retardant particles is too large, which leads to a decrease in its activity and a worse flame retardant effect; in addition, large-particle-size flame retardants will block the electronic pathway, increase electrode polarization, and reduce the performance of electrochemical properties.
[0039] Preferably, the areal density of the flame-retardant layer is 3.9-21 g / cm³. 2 The density of the flame-retardant layer is less than 3.9 g / cm³. 2 The flame retardant content is insufficient, resulting in poor flame retardant performance. The density of the flame-retardant layer is greater than 21 g / cm³. 2 Excessive use of flame retardants reduces the energy density of the battery cell.
[0040] Preferably, in the above-mentioned flame-retardant layer, the mass ratio of flame-retardant material, conductive material, and binder is (3-6):(3-6):1. If the content of flame-retardant material is too low, such as 1:8:1, the flame-retardant effect is poor. If the content of flame-retardant is too high, such as 6:2:1, the electronic conductivity of the flame-retardant layer is poor, which will increase the internal resistance of the battery cell and reduce the capacity utilization of the battery cell.
[0041] Preferably, the flame-retardant material in the flame-retardant layer includes at least one of antimony trioxide, brominated polystyrene, aluminum hydroxide, magnesium hydroxide, and ammonium polyphosphate.
[0042] Preferably, the conductive material in the flame-retardant layer includes at least one of carbon nanotubes, graphene, and conductive carbon black.
[0043] Preferably, the binder in the flame-retardant layer includes at least one of polyethylene oxide, polytetrafluoroethylene, polyacrylic acid, sodium hydroxymethyl cellulose, and styrene-butadiene rubber.
[0044] This application does not impose specific limitations on the positive electrode current collector, which can be any positive electrode current collector in the art. As an example, the positive electrode current collector includes aluminum foil.
[0045] This application does not impose specific limitations on the positive electrode material layer, and any positive electrode material layer in the art can be selected. As an example, the positive electrode material layer includes a positive electrode material, a conductive material, and a binder, with a mass ratio of (90-95):(5-10):5. The positive electrode material includes lithium iron phosphate, lithium manganese oxide, lithium cobalt oxide, and ternary lithium storage materials (LiNi). x Co y Mn z At least one of O2, x+y+z=1); the conductive material includes at least one of carbon nanotubes, graphene, and conductive carbon black; the binder includes at least one of polyethylene oxide, polytetrafluoroethylene, polyacrylic acid, sodium hydroxymethyl cellulose, and styrene-butadiene rubber.
[0046] Optionally, the areal density of the positive electrode material layer is 150 g / cm³. 2 .
[0047] Optionally, a flame-retardant layer and a positive electrode material layer are provided on the positive electrode current collector side, as shown in the schematic diagram. Figure 1 .
[0048] Optionally, a flame-retardant layer and a positive electrode material layer are provided on both sides of the positive electrode current collector.
[0049] According to a second aspect of this application, a method for preparing the above-mentioned positive electrode sheet is provided, comprising the following steps:
[0050] Flame-retardant materials, conductive materials, and binders are dispersed in a solvent to obtain a flame-retardant slurry;
[0051] The flame-retardant slurry is coated onto at least one side of the current collector, and then subjected to a first drying process to form a flame-retardant layer;
[0052] A positive electrode material slurry is coated on the side of the flame-retardant layer facing away from the current collector, and then a second drying process is performed to obtain a positive electrode sheet.
[0053] Preferably, a rolling process is performed after the first drying and before coating the positive electrode material layer slurry. This not only reduces the porosity of the flame-retardant layer and increases the contact area between the flame-retardant material and the conductive material, thus enhancing electron transport capability, but also reduces the thickness of the inactive components, significantly improving the overall energy density of the battery cell.
[0054] Preferably, the solid content of the flame-retardant slurry is 5wt.%-20wt.%, such as 5wt.%, 10wt.%, 15wt.%, or 20wt.%.
[0055] Preferably, the solvent in the flame-retardant slurry includes at least one of N-methylpyrrolidone (NMP), deionized water, and ethanol.
[0056] This application does not impose specific limitations on the first drying method described above, and any method of drying the flame-retardant layer in this field can be used, such as baking, air drying, or sun drying.
[0057] This application does not impose specific limitations on the cathode material layer slurry; any cathode material layer slurry in the art can be used. As an example, the cathode material layer slurry includes a cathode material, a conductive material, a binder, and a solvent. The solid content of the cathode material layer slurry is 55 wt.%, and the mass ratio of the cathode material, conductive material, and binder is 90:5:5. The cathode material includes lithium iron phosphate, lithium manganese oxide, lithium cobalt oxide, and ternary lithium storage materials (LiNi). x Co y Mn z O2, where x+y+z=1; x=0~1, such as x=0, 0.001, 0.005, 0.01, 0.05, 0.09 or 0.1 etc.; y=0~1, such as y=0, 0.001, 0.005, 0.01, 0.05, 0.09 or 0.1 etc.; z=0~1, such as z=0, 0.001, 0.005, 0.01, 0.05, 0.09 or 0.1 etc.; conductive material includes at least one of carbon nanotubes, graphene, conductive carbon black; binder includes at least one of polyethylene oxide, polytetrafluoroethylene, polyacrylic acid, sodium carboxymethyl cellulose, styrene-butadiene rubber; solvent includes at least one of polyethylene oxide, polytetrafluoroethylene (PTFE), polyacrylic acid, sodium carboxymethyl cellulose, styrene-butadiene rubber.
[0058] This application does not impose specific limitations on the above-mentioned second drying method, and any drying method of the positive electrode material layer in this field can be adopted, such as baking, air drying, or drying.
[0059] After the second drying process described above, rolling treatment may or may not be performed.
[0060] According to a third aspect of this application, a secondary battery is provided, comprising the above-described positive electrode sheet or the positive electrode sheet prepared by the above-described preparation method.
[0061] According to a fourth aspect of this application, an electrical device is provided, including the aforementioned secondary battery. This application does not specifically limit the electrical device; as an example, the electrical device includes at least one of an electric vehicle, a residential energy storage device, and an industrial / commercial energy storage device.
[0062] The present application will be further described below with reference to specific embodiments.
[0063] Example 1
[0064] Flame retardant material, conductive material and binder are dispersed in solvent at a mass ratio of 4.5:4.5:1 to obtain a flame retardant slurry with a solid content of 10 wt.%. The flame retardant material is antimony trioxide with a primary particle size D50 of 1500 nm, the conductive material is carbon nanotubes with a primary particle size D50 of 2000 nm, the binder is polyethylene oxide, and the solvent is NMP.
[0065] The obtained flame-retardant slurry was coated on both sides of the aluminum foil, dried first, and then rolled to form an areal density of 10 g / cm³. 2 And the compaction density is 1 g / cm³ 3 Flame-retardant layer;
[0066] A cathode material, a conductive material, and a binder are dispersed in a solvent at a mass ratio of 90:5:5 to obtain a cathode material slurry with a solid content of 55 wt.%. The cathode material is lithium iron phosphate, the conductive material is carbon nanotubes, the binder is polyethylene oxide, and the solvent is NMP.
[0067] The obtained positive electrode material slurry is coated onto the flame-retardant layer on the surface away from the aluminum foil and then dried a second time to form an areal density of 150 g / cm³. 2 The positive electrode material layer is used to obtain the positive electrode sheet.
[0068] Example 2
[0069] The difference from Example 1 is that, in this example, the flame retardant material used in preparing the flame retardant layer slurry is antimony trioxide with a primary particle size D50 of 1200 nm.
[0070] Example 3
[0071] The difference from Example 1 is that, in this example, the flame retardant material used in the preparation of the flame retardant layer slurry is antimony trioxide with a primary particle size D50 of 1800 nm.
[0072] Example 4
[0073] The difference from Example 1 is that, in this example, when preparing the flame-retardant layer slurry, the flame-retardant material used is antimony trioxide with a primary particle size of D50 60nm, and the conductive material is carbon nanotubes with a primary particle size of D50 100nm.
[0074] Example 5
[0075] The difference from Example 1 is that, in this example, when preparing the flame retardant layer slurry, the flame retardant material used is antimony trioxide with a primary particle size D50 of 3000 nm, and the conductive material is carbon nanotubes with a primary particle size D50 of 4000 nm.
[0076] Example 6
[0077] The difference from Example 1 is that the pressure of the roller pressing before coating the positive electrode material layer slurry is adjusted in this example to make the compaction density of the flame retardant layer 0.2 g / cm³. 3 .
[0078] Example 7
[0079] The difference from Example 1 is that the pressure of the roller pressing before coating the positive electrode material layer slurry is adjusted in this example to make the compaction density of the flame retardant layer 2 g / cm³. 3 .
[0080] Example 8
[0081] The difference from Example 1 is that the amount of flame-retardant slurry applied in this example is adjusted to achieve an areal density of 4 g / cm³. 2 .
[0082] Example 9
[0083] The difference from Example 1 is that the amount of flame-retardant slurry applied in this example is adjusted to achieve an areal density of 20 g / cm³. 2 .
[0084] Example 10
[0085] The difference from Example 1 is that, in this example, when preparing the flame-retardant layer slurry, the flame-retardant material used is brominated polystyrene with a primary particle size D50 of 1500 nm, the conductive material is graphene with a primary particle size D50 of 2000 nm, the binder is PTFE, and the solvent is deionized water.
[0086] Example 11
[0087] The difference from Example 1 is that, in this example, when preparing the flame retardant slurry, the flame retardant material used is aluminum hydroxide with a primary particle size D50 of 1500 nm, the conductive material is conductive carbon black with a primary particle size D50 of 2000 nm, the binder is polyacrylic acid, and the solvent is ethanol.
[0088] Example 12
[0089] The difference from Example 1 is that, in this example, when preparing the flame retardant slurry, the flame retardant material used is magnesium hydroxide with a primary particle size D50 of 1500 nm, the conductive material is carbon nanotubes with a primary particle size D50 of 2000 nm, the binder is sodium carboxymethyl cellulose, and the solvent is NMP.
[0090] Example 13
[0091] The difference from Example 1 is that in this example, when preparing the flame retardant slurry, the flame retardant material used is ammonium polyphosphate with a primary particle size D50 of 1500 nm, the conductive material is carbon nanotubes with a primary particle size D50 of 2000 nm, the binder is styrene-butadiene rubber, and the solvent is NMP.
[0092] Example 14
[0093] The difference from Example 1 is that in this example, the mass ratio of flame retardant material, conductive material and binder used in the preparation of the flame retardant slurry is 3:6:1, and the solid content of the resulting flame retardant slurry is 5 wt.%.
[0094] Example 15
[0095] The difference from Example 1 is that in this example, the mass ratio of flame retardant material, conductive material and binder used in the preparation of the flame retardant slurry is 6:3:1, and the solid content of the resulting flame retardant slurry is 20 wt.%.
[0096] Comparative Example 1
[0097] The difference from Example 1 is that the flame retardant material used in this comparative example when preparing the flame retardant layer slurry is antimony trioxide with a primary particle size of D50 500nm.
[0098] Comparative Example 2
[0099] The difference from Example 1 is that the flame retardant material used in this comparative example when preparing the flame retardant layer slurry is antimony trioxide with a primary particle size D50 of 3000nm.
[0100] Comparative Example 3
[0101] The difference from Example 1 is that the rolling pressure before coating the positive electrode material layer slurry in this comparative example is adjusted to achieve a compaction density of 4.0 g / cm³ for the flame-retardant layer. 3 .
[0102] Comparative Example 4
[0103] The difference from Example 1 is that this comparative example did not undergo rolling after the first drying and before coating the positive electrode material layer slurry, resulting in a compacted density of 0.05 g / cm³ for the flame-retardant layer. 3 .
[0104] The battery cells assembled and tested according to the above embodiments and comparative examples are as follows:
[0105] Flame retardant effect test: The flame retardant effect of the battery cell is evaluated by needle penetration test. The quality of the flame retardant effect is judged based on whether it catches fire.
[0106] Electrochemical performance testing: A constant current testing scheme was used to evaluate the discharge capacity of the battery at a current density of 1C, and the volumetric energy density (Wh / L) of the cell was calculated based on the electrode thickness.
[0107] The electron transport of the battery cell is evaluated by DC resistance testing. The higher the internal resistance of the battery cell, the stronger the suppression effect of the feedback flame retardant layer on electron transport.
[0108] The negative electrode material in the cell is graphite, the electrolyte is 1.0M LiPF6 in EC / DEC, the designed capacity is 50Ah, and the cell form is a stacked soft-pack battery.
[0109] The test results are shown in Table 1.
[0110] Table 1. Summary of Flame Retardancy and Cell Performance
[0111]
[0112] As can be seen from the above data, all embodiments of this application passed the flame retardant test, and the cell volumetric energy density was above 393Wh / L, and the cell internal resistance was below 0.39mΩ. Comparative Example 1 had poor flame retardancy due to an excessively small D2 / D1 ratio; Comparative Example 2 had an excessively large D2 / D1 ratio, which caused the flame retardant particles to block the electron transmission channel, resulting in a high cell internal resistance; Comparative Example 3 failed the flame retardant test because the compaction density of the flame retardant layer was too high; and Comparative Example 4 had a low compaction density, resulting in a low cell volumetric energy density and a high internal resistance.
[0113] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application and are not intended to limit the scope of protection of this application. Although this application has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of this application without departing from the substance and scope of the technical solutions of this application.
Claims
1. A positive electrode plate, characterized in that, It includes a current collector, and a flame retardant layer is provided on at least one side of the current collector, and a positive electrode material layer is provided on the surface of the flame retardant layer opposite to the current collector; The flame-retardant layer comprises a flame-retardant material, a conductive material, and an adhesive, and satisfies the following relationship: 1 / 2D1 < D2 <D1, Wherein, D1 is the primary particle size D50 of the conductive material in the flame-retardant layer. D2 is the primary particle size D50 of the flame-retardant material in the flame-retardant layer; The compacted density of the flame-retardant layer is 0.19-2.1 g / cm³. 3 .
2. The positive electrode sheet as described in claim 1, characterized in that, D2 / D1=0.
75.
3. The positive electrode sheet as described in claim 1, characterized in that, D1=90-4100 nm, D2=40-3100 nm.
4. The positive electrode sheet as described in claim 1, characterized in that, In the flame-retardant layer, the mass ratio of flame-retardant material, conductive material and binder is (3-6):(3-6):
1.
5. The positive electrode sheet as described in claim 1, characterized in that, It also satisfies at least one of features a)-c): a) The flame-retardant material in the flame-retardant layer includes at least one of antimony trioxide, brominated polystyrene, aluminum hydroxide, magnesium hydroxide, and ammonium polyphosphate; b) The conductive material in the flame-retardant layer includes at least one of carbon nanotubes, graphene, and conductive carbon black; c) The binder in the flame-retardant layer includes at least one of polyethylene oxide, polytetrafluoroethylene, polyacrylic acid, sodium hydroxymethyl cellulose, and styrene-butadiene rubber.
6. A method for preparing a positive electrode sheet as described in claim 1, characterized in that, Includes the following steps: Flame-retardant materials, conductive materials, and binders are dispersed in a solvent to obtain a flame-retardant slurry; The flame-retardant slurry is coated onto at least one side of the current collector, rolled, and then dried to form a flame-retardant layer. A positive electrode material slurry is coated on the surface of the flame-retardant layer facing away from the current collector, and then a second drying process is performed to obtain a positive electrode sheet.
7. A secondary battery, characterized in that, This includes the positive electrode sheet as described in any one of claims 1 to 5 or the positive electrode sheet prepared by the preparation method as described in claim 6.
8. An electrical appliance, characterized in that, Includes the secondary battery as described in claim 7.
Citation Information
Patent Citations
Lightweight flame-retardant current collector, preparation method thereof, electrode and battery
CN114156486A
Positive plate, preparation method thereof and secondary battery
CN115472770A