Biological stent, biological stent preform and method for preparing the same
By preparing pre-made bioscaffolds of polylactic acid and polylactic acid-polycaprolactone copolymer and grafting gelatin, the problems of fistula and stenosis caused by the inertness of ureteral stent materials were solved, achieving high toughness and good biocompatibility, and promoting urothelial cell adhesion and tissue regeneration.
Patent Information
- Application Number
- CN202410137600.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-19
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-07-19
AI Technical Summary
Existing ureteral stent materials are prone to fistula formation and stenosis due to inertness, and the urothelial reconstruction effect is not ideal, affecting the adhesion and movement of urothelial cells, leading to ureteral fibrosis and stenosis.
A pre-formed PP scaffold was prepared using polylactic acid and polylactic acid-polycaprolactone copolymer via thermally induced phase separation. Gelatin was then grafted onto the scaffold using ammonolysis and glutaraldehyde crosslinking to form a PP-gel scaffold, which improves biocompatibility and hydrophilicity, making it suitable for the clinical treatment of long ureteral defects.
PP-gel stents have high toughness and good biocompatibility, promote the adhesion and proliferation of urinary epithelial cells, are suitable for the clinical treatment of long ureteral defects, prevent fibrosis and stenosis, and support tissue regeneration.
Smart Images

Figure CN117982738B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of biomedical materials, and in particular to a biological scaffold for tubular tissues, a biological scaffold preform, and a method for preparing the same. Background Technology
[0002] Any ureteral disease, such as internal factors like stones, tumors, or malformations, or external factors like injury, infection, or inflammation, can cause ureteral obstruction, leading to hydronephrosis or kidney damage, severely impacting the patient's physical and mental health. Especially when there are long segments of abnormalities or lesions in the ureter, it poses a significant challenge for urologists. Currently, procedures such as kidney transplantation, ureterocystostomy, ureteroileal replacement, and ureterostomy are not always successful, and face challenges such as serious complications, anastomotic stenosis, chronic renal failure, and donor tissue collection. In short, the clinical treatment of long ureteral defects still faces various challenges.
[0003] With technological advancements, ureteral tissue engineering has gained a foothold as a potential alternative to autologous transplantation. Various natural and synthetic polymers, such as collagen, silk fibroin, gelatin, polylactic acid, and polycaprolactone, are commonly used in ureteral stents. However, on the one hand, the formation of fistulas and stenosis due to stent inertia leads to less than ideal ureteral repair outcomes. On the other hand, ureteral repair is a complex process involving the reconstruction of the urothelial layer and smooth muscle layer. The urothelial layer acts as a barrier, protecting underlying tissues from toxic components in urine, which can lead to ureteral fibrosis, constriction, and stenosis. Furthermore, different stents can affect the adhesion and movement of urothelial cells.
[0004] Therefore, for the fields of urology and tissue engineering, researching more suitable stents is of great significance for the treatment of ureteral diseases. Summary of the Invention
[0005] One object of the present invention is to provide a biological scaffold, a biological scaffold preform, and a method for preparing the same. The biological scaffold is prepared by first obtaining a biological scaffold preform (PP scaffold) from polylactic acid and polylactic acid-polycaprolactone copolymer, and then grafting gelatin to obtain a PP-gel scaffold. The PP-gel scaffold has high toughness and good biocompatibility, and has great potential for clinical application.
[0006] Another objective of this invention is to provide a biological scaffold, a biological scaffold preform, and a method for preparing the same, which is prepared by using a thermally induced phase separation method and an ammonolytic GA crosslinking method, and the operation is simple.
[0007] Another objective of this invention is to provide a biological scaffold, a biological scaffold preform, and a method for preparing the same. The prepared biological scaffold has strong hydrophilicity, which helps the adhesion and proliferation of urinary epithelial cells, making it suitable as an ideal scaffold for clinical treatment of long ureteral defects.
[0008] Another objective of this invention is to provide a biological scaffold, a biological scaffold preform, and a method for preparing the same. The biological scaffold has strong biocompatibility and can be prepared using different molds to be suitable for use in various organs. It can be applied to the treatment of related organ diseases in the human body.
[0009] Another objective of this invention is to provide a biological scaffold, a biological scaffold preform, and a method for preparing the same, wherein the biological scaffold prepared by thermal phase separation has ideal porosity and pore size on both its surface and interior, making it highly suitable for clinical application as a biological scaffold.
[0010] Another object of the present invention is to provide a biological scaffold, a biological scaffold preform and a method for preparing the same, wherein the biological scaffold has a porous and dense surface, which is conducive to epithelial formation and at the same time can prevent cells from entering the scaffold.
[0011] Another object of the present invention is to provide a biological scaffold, a biological scaffold preform and a method for preparing the same, wherein the biological scaffold has high porosity and large pores, and such a physical structure allows cell migration and nutrient circulation, which is beneficial for promoting tissue regeneration.
[0012] Another objective of this invention is to provide a biological scaffold, a pre-form of the biological scaffold, and a method for preparing the same. The PP46-gel biological scaffold has optimal porosity and pore size, which not only facilitates nutrient circulation but also has anti-fibrotic effects. Therefore, the biological scaffold can be implanted into the ureter, which can significantly improve the healing of the urinary tract epithelium and delay the decline of renal function, making it suitable for clinical application.
[0013] According to one aspect of the present invention, a method for preparing a biological scaffold is provided, comprising the following steps:
[0014] (A) Preparation of biological materials using polylactic acid / polylactic acid-polycaprolactone copolymer (PLLA / PLCL) as raw material
[0015] Prefabricated PP brackets; and
[0016] (B) Grafted gelatin: gelatin is fixed to the above PP scaffold using ammonolysis and glutaraldehyde (GA) crosslinking method to obtain PP-gel scaffold.
[0017] In step (A), the mass ratio of PLLA to PLCL is in the range of 1:9 to 9:1.
[0018] The following steps are used to prepare the PP scaffold:
[0019] (A1) Preparation of homogeneous polylactic acid / polylactic acid-polycaprolactone copolymer (PLLA / PLCL) polymer
[0020] Solution;
[0021] (A2) Pour the above polymer solution into a preheated mold;
[0022] (A3) Phase separation, freeze-drying to obtain PP scaffold;
[0023] In step (A1), PLLA and PLCL are dissolved in 1,4-dioxane at 65°C in mass ratios of 1:9, 2:8, 3:7, 4:6, 5:5, 6:4, 7:3, 8:2 and 9:1 respectively to form a homogeneous polymer solution. In step (A3), the polymer solution and the mold are placed at -80°C for 24 hours and then freeze-dried for 72 hours to obtain the PP scaffold.
[0024] In step (A1), PLLA and PLCL are dissolved in 1,4-dioxane at 65°C according to a predetermined mass ratio to form a homogeneous polymer solution. In step (A3), the polymer solution and the mold are placed at -80°C for 24 hours and then freeze-dried for 72 hours to obtain a PP scaffold.
[0025] Step (B) includes the following steps:
[0026] Impurities are removed by soaking and drying;
[0027] Aldehyde-modified scaffolds were prepared by ammonolysis and glutaraldehyde crosslinking; and
[0028] PP-gel scaffolds were obtained by grafting gelatin.
[0029] The step (B) mentioned above includes the following steps:
[0030] (B1) The PP scaffold was soaked in 95% alcohol for 1 hour, then dried in a vacuum oven, and further soaked in 0.06 g / ml 1,6-hexanediamine / isopropanol solution for 10 minutes, and then rinsed with plenty of water to remove free hexanediamine, thereby obtaining a scaffold with impurities removed.
[0031] (B2) The aminated PP scaffold was soaked in a 1.0 wt% GA aqueous solution at room temperature for 3 h, and then rinsed with plenty of water to remove free GA, thus obtaining an aldehyde-modified scaffold.
[0032] (B3) The aldehyde-modified scaffold was incubated in 1.0 wt% gelatin / PBS solution at room temperature for 24 h, and then the ungrafted gelatin was washed away with water to obtain the PP-gel scaffold.
[0033] In step (A3), the PP support is manufactured into a tubular support or a circular support using a matching mold.
[0034] In step (A1), the mass ratio of PLLA to PLCL is 4:6.
[0035] The PP-gel stent is manufactured using ureteral stent molds, intestinal stent molds, esophageal stent molds, urethral stent molds, gastric tube stent molds, or vascular stent molds to obtain the ureteral stent, intestinal stent, esophageal stent, urethral stent, gastric tube stent, or vascular stent required for clinical use.
[0036] According to another aspect of the present invention, the present invention also provides a biological scaffold, including a ureteral scaffold, an intestinal scaffold, an esophageal scaffold, a urethral scaffold, or a vascular scaffold, wherein the biological scaffold is prepared by the following method:
[0037] (A) Prepare a homogeneous polymer solution of polylactic acid / polylactic acid-polycaprolactone copolymer (PLLA / PLCL) with a concentration of 10% (w / v);
[0038] (B) Pour the above polymer solution into a preheated mold;
[0039] (C) Phase separation and freeze-drying yielded a PP scaffold; and
[0040] (D) Grafted gelatin: gelatin is fixed to the above PP scaffold by ammonolysis and glutaraldehyde (GA) crosslinking to obtain a PP-gel scaffold with high micropores and high hydrophilicity.
[0041] The present invention also provides a biological scaffold, wherein the biological scaffold includes a ureteral scaffold, an intestinal scaffold, an esophageal scaffold, a urethral scaffold, or a vascular scaffold, characterized in that the biological scaffold comprises the following materials: polylactic acid, polylactic acid-polycaprolactone copolymer, and gelatin.
[0042] The present invention also provides a biological scaffold preform, wherein the biological scaffold preform is manufactured by using a ureteral scaffold mold, an intestinal scaffold mold, an esophageal scaffold mold, a urethral scaffold mold or a vascular scaffold mold to obtain the clinically required ureteral scaffold, intestinal scaffold, esophageal scaffold, urethral scaffold or vascular scaffold
[0043] The biological scaffold preform mentioned above is prepared using the following method:
[0044] (A1) Preparation of homogeneous polylactic acid / polylactic acid-polycaprolactone copolymer (PLLA / PLCL) polymer
[0045] Solution;
[0046] (A2) Pour the above polymer solution into a preheated mold; and
[0047] (A3) Phase separation, freeze-drying to obtain PP scaffold. Attached Figure Description
[0048] Figure 1 This is an ammonolysis crosslinking reaction process of a PP-gel scaffold according to an embodiment of the present invention.
[0049] Figure 2 This is an electron microscope image of a PP46 scaffold prepared according to the fourth embodiment of the present invention.
[0050] Figure 3 This is an electron microscopy (SEM) image analysis of nine types of PP scaffolds prepared according to nine embodiments of the present invention.
[0051] Figure 4 These are analytical diagrams of the pore size, pore diameter, and porosity of PP stents with different specific gravities according to various embodiments of the present invention.
[0052] Figure 5 The results are based on the contact angle image analysis of the PP46 and PP46-gel scaffolds prepared according to the fourth embodiment of the present invention.
[0053] Figure 6 The figure shows the stress-strain curves of PP46 and PP46-gel according to the fourth embodiment of the present invention.
[0054] Figure 7 The image shows the total reflectance infrared spectra of PP46 and PP46-gel with gelatin powder according to the fourth embodiment of the present invention.
[0055] Figure 8 The images shown are images of epithelial cell proliferation results according to at least one embodiment and a comparative embodiment of the present invention.
[0056] Figure 9 The results shown are from animal experiments involving subcutaneous implantation according to at least one embodiment and a comparative embodiment of the present invention.
[0057] Figure 10 The images shown are of stents after transplantation according to at least one embodiment and a comparative embodiment of the present invention.
[0058] Figure 11 The figures shown are the results of urothelialization phenotypes in at least one embodiment and a comparative embodiment according to the present invention.
[0059] Figure 12 The results are based on protein expression studies according to at least one embodiment and comparative embodiment of the present invention. Detailed Implementation
[0060] The following description is intended to disclose the present invention and enable those skilled in the art to implement it. The preferred embodiments described below are merely examples, and other obvious variations will occur to those skilled in the art. The basic principles of the invention defined in the following description can be applied to other embodiments, modifications, improvements, equivalents, and other technical solutions that do not depart from the spirit and scope of the invention.
[0061] Gelatin is a natural protein, a partially hydrolyzed product of collagen, containing an integrin-aspartic acid (RGD) peptide sequence and is commonly used in tissue engineering. However, due to its low mechanical properties, gelatin makes surgical reconstruction of the ureter difficult; therefore, it is necessary to graft various synthetic polymers. Polylactic acid (PLLA) is a commonly used polymer that can be fabricated into nanofiber porous scaffolds using thermally induced phase separation (TIPS). However, PLLA is rigid and brittle, making ureteral remodeling difficult when used in ureteral scaffolds. Therefore, we combined PLLA with polylactic acid-polycaprolactone copolymer (PLCL), which has good elasticity. However, due to the poor hydrophobicity and cell adhesion of synthetic polyesters, they cannot properly regulate cell phenotype. Therefore, we chose to graft natural gelatin to increase the hydrophilicity and cell adhesion of the scaffold.
[0062] In this invention, gelatin materials are chemically modified using polylactic acid / polylactic acid-polycaprolactone copolymer (PLLA / PLCL) mixtures in different proportions, and a highly microporous tubular scaffold with a thermally induced phase separation (TIPS) topology is created. In other words, this invention prepares a PLLA / PLCL scaffold, i.e., a PP scaffold, using thermally induced phase separation (TIPS). The effects of gelatin-modified synthetic materials on abnormalities in long ureters are then investigated, exploring the transduction of biological signals in the channels accompanying the application of gelatin synthetic materials as biological scaffolds. This provides a new scaffold material and manufacturing method for ureteral scaffolds. Therefore, the scaffold in this invention can be used in ureteral tissue engineering and can be applied to various small-diameter tubular tissues in different organs in the future.
[0063] This invention employs hexamethylenediamine ammonolysis and glutaraldehyde crosslinking to graft gelatin onto a polymer ester. (See attached figures) Figure 1 This describes the experimental procedure for preparing PP46-gel scaffolds via ammonolysis and GA crosslinking. Specifically, ester bonds in the material are broken by amino groups, the scaffold surface is aldehyde-modified with excess GA, and finally, the amino groups on the gelatin undergo a Schiff base reaction with the scaffold surface for crosslinking.
[0064] The biological scaffold of the present invention, its preparation materials, and its preparation method are further described below with reference to specific embodiments.
[0065] Materials and reagents:
[0066] Polylactic acid (PLLA) (MW = 20 kDa), purchased from Ningbo Institute of Materials Technology and Engineering;
[0067] Polylactic acid-polycaprolactone copolymer (PLCL) (50:50, MW=30kDa) was purchased from Jinan Daigang Bioengineering Co., Ltd., China.
[0068] 1,4-Dioxane, hexamethylenediamine (HMD) and glutaraldehyde (GA) were purchased from Aladdin Reagents Co., Ltd. (Shanghai, China).
[0069] Gelatin, purchased from Sigma-Aldrich (Missouri, USA).
[0070] Example 1:
[0071] (A) PLLA and PLCL in a mass ratio of 1:9 were dissolved in 1,4-dioxane at 65°C to form a homogeneous polymer solution with a concentration of 10% (w / v).
[0072] (B) Pour into a preheated mold;
[0073] (C) Phase separation: The polymer solution and the mold were placed at -80°C for 24 hours and then freeze-dried for 72 hours to obtain the biological scaffold preform - PP19 scaffold.
[0074] (D) Grafted gelatin: gelatin was fixed to the above PP19 scaffold using ammonolysis and glutaraldehyde (GA) crosslinking method to obtain PP19-gel scaffold.
[0075] In step (C), the PP19 scaffold can be a tubular scaffold or a circular scaffold, wherein the circular scaffold is fabricated in a steel mold (60 mm in diameter and 1 mm in height). Additionally, in step (C), thermally induced phase separation is used to prepare the biological scaffold preform.
[0076] In step (D), step (D) includes the following steps:
[0077] (D1) Removal of impurities: The PP19 support was soaked in 95% alcohol for 1 hour, then dried in a vacuum oven, and further soaked in 0.06 g / ml 1,6-hexanediamine / isopropanol solution for 10 minutes, and then rinsed with plenty of water to remove free hexanediamine.
[0078] (D2) Aldehyde-modified scaffold: The PP19 scaffold was immersed in a 1.0 wt% GA aqueous solution at room temperature for 3 hours, and then rinsed with plenty of water to remove free GA;
[0079] (D3) Grafted gelatin: The above aldehyde-modified scaffold was cultured in 1.0 wt% gelatin / PBS solution at room temperature for 24 h, and then the ungrafted gelatin was washed away with water to obtain the PP19-gel scaffold.
[0080] The step (D1) mentioned above is to remove impurities from step (C) before grafting gelatin.
[0081] In step (A), a 10% w / v homogeneous polymer solution is formed.
[0082] The PP19 scaffolds prepared in steps (A), (B), and (C) are used as pre-made biological scaffolds for subsequent grafting of gelatin.
[0083] The procedure further includes a step (E) of manufacturing the PP19-gel scaffold into a biological scaffold for clinical application using a corresponding mold.
[0084] Example 2:
[0085] (A) PLLA and PLCL in a mass ratio of 2:8 were dissolved in 1,4-dioxane at 65°C to form a homogeneous polymer solution with a concentration of 10% (w / v).
[0086] (B) Pour into a preheated mold;
[0087] (C) Phase separation: The polymer solution and the mold were placed at -80°C for 24 hours and then freeze-dried for 72 hours to obtain the PP28 scaffold.
[0088] (D) Grafted gelatin: gelatin was fixed to the above PP28 scaffold using ammonolysis and glutaraldehyde (GA) crosslinking method to obtain PP28-gel scaffold.
[0089] In step (C), the PP28 scaffold can be a tubular scaffold or a circular scaffold, wherein the circular scaffold is fabricated in a steel mold (60 mm in diameter and 1 mm in height). Additionally, in step (C), thermally induced phase separation is used to prepare the biological scaffold preform.
[0090] In step (D), step (D) includes the following steps: (D1) removing impurities; (D2) aldehyde-based scaffold; and (D3) grafting gelatin. The specific operations of steps (D1)-(D3) are all as described in Example 1.
[0091] In step (A), a 10% w / v homogeneous polymer solution is formed.
[0092] The PP28 scaffolds obtained in steps (A), (B), and (C) are used as pre-made biological scaffolds for subsequent grafting of gelatin.
[0093] The procedure further includes a step (E) in which the PP28-gel scaffold is manufactured into a biological scaffold for clinical application using a corresponding mold.
[0094] Example 3:
[0095] (A) PLLA and PLCL in a mass ratio of 3:7 were dissolved in 1,4-dioxane at 65°C to form a homogeneous polymer solution with a concentration of 10% (w / v);
[0096] (B) Pour into a preheated mold;
[0097] (C) Phase separation: The polymer solution and the mold were placed at -80°C for 24 hours and then freeze-dried for 72 hours to obtain the PP37 scaffold.
[0098] (D) Grafted gelatin: gelatin was fixed to the above PP37 scaffold using ammonolysis and glutaraldehyde (GA) crosslinking method to obtain PP37-gel scaffold.
[0099] In step (C), the PP37 bracket can be a tubular bracket or a circular bracket, wherein the circular bracket is manufactured in a steel mold (60mm in diameter and 1mm in height).
[0100] In step (D), step (D) includes the following steps: (D1) removing impurities; (D2) aldehyde-based scaffold; and (D3) grafting gelatin. The specific operations of steps (D1)-(D3) are all as described in Example 1.
[0101] In step (A), a 10% w / v homogeneous polymer solution is formed.
[0102] The PP37 scaffolds obtained in steps (A), (B), and (C) are used as pre-made biological scaffolds for subsequent grafting of gelatin.
[0103] In addition, in step (C), the biological scaffold preform is prepared by thermally induced phase separation.
[0104] The procedure further includes a step (E) of manufacturing the PP37-gel scaffold into a biological scaffold for clinical application using a corresponding mold.
[0105] Example 4:
[0106] (A) PLLA and PLCL in a mass ratio of 4:6 were dissolved in 1,4-dioxane at 65°C to form a homogeneous polymer solution;
[0107] (B) Pour into a preheated mold;
[0108] (C) Phase separation: The polymer solution and the mold were placed at -80°C for 24 hours and then freeze-dried for 72 hours to obtain the PP46 scaffold.
[0109] (D) Grafted gelatin: gelatin was fixed to the above PP46 scaffold using ammonolysis and glutaraldehyde (GA) crosslinking method to obtain PP46-gel scaffold.
[0110] In step (C), the PP46 scaffold can be a tubular scaffold or a circular scaffold, wherein the circular scaffold is fabricated in a steel mold (60 mm in diameter and 1 mm in height). Additionally, in step (C), thermally induced phase separation is used to prepare the biological scaffold preform.
[0111] In step (D), step (D) includes the following steps: (D1) removing impurities; (D2) aldehyde-based scaffold; and (D3) grafting gelatin. The specific operations of steps (D1)-(D3) are all as described in Example 1.
[0112] In step (A), a 10% w / v homogeneous polymer solution is formed.
[0113] The PP46 scaffolds obtained in steps (A), (B), and (C) are used as pre-made biological scaffolds for subsequent grafting of gelatin.
[0114] The procedure further includes a step (E) of manufacturing the PP46-gel scaffold into a biological scaffold for clinical application using a corresponding mold.
[0115] Example 5:
[0116] (A) PLLA and PLCL in a mass ratio of 5:5 were dissolved in 1,4-dioxane at 65°C to form a homogeneous polymer solution with a concentration of 10% (w / v).
[0117] (B) Pour into a preheated mold;
[0118] (C) Phase separation: The polymer solution and the mold were placed at -80°C for 24 hours and then freeze-dried for 72 hours to obtain the PP55 scaffold.
[0119] (D) Grafted gelatin: gelatin is fixed to the above PP55 scaffold by ammonolysis and glutaraldehyde (GA) crosslinking method to obtain PP55-gel scaffold.
[0120] In step (C), the PP55 scaffold can be a tubular scaffold or a circular scaffold, wherein the circular scaffold is fabricated in a steel mold (60 mm in diameter and 1 mm in height). Additionally, in step (C), thermally induced phase separation is used to prepare the biological scaffold preform.
[0121] In step (D), step (D) includes the following steps: (D1) removing impurities; (D2) aldehyde-based scaffold; and (D3) grafting gelatin. The specific operations of steps (D1)-(D3) are all as described in Example 1.
[0122] In step (A), a 10% w / v homogeneous polymer solution is formed.
[0123] The PP55 scaffolds prepared in steps (A), (B), and (C) are used as pre-made biological scaffolds for subsequent grafting of gelatin.
[0124] The procedure further includes a step (E) of manufacturing the PP55-gel scaffold into a biological scaffold for clinical application using a corresponding mold.
[0125] Example 6:
[0126] (A) PLLA and PLCL in a mass ratio of 6:4 were dissolved in 1,4-dioxane at 65°C to form a homogeneous polymer solution with a concentration of 10% (w / v).
[0127] (B) Pour into a preheated mold;
[0128] (C) Phase separation: The polymer solution and the mold were placed at -80°C for 24 hours and then freeze-dried for 72 hours to obtain the PP64 scaffold.
[0129] (D) Grafted gelatin: gelatin was fixed to the above PP64 scaffold by ammonolysis and glutaraldehyde (GA) crosslinking to obtain PP64-gel scaffold.
[0130] In step (C), the PP64 scaffold can be a tubular scaffold or a circular scaffold, wherein the circular scaffold is fabricated in a steel mold (60 mm in diameter and 1 mm in height). Additionally, in step (C), thermally induced phase separation is used to prepare the biological scaffold preform.
[0131] In step (D), step (D) includes the following steps: (D1) removing impurities; (D2) aldehyde-based scaffold; and (D3) grafting gelatin. The specific operations of steps (D1)-(D3) are all as described in Example 1.
[0132] In step (A), a 10% w / v homogeneous polymer solution is formed.
[0133] The PP64 scaffolds obtained in steps (A), (B), and (C) are used as pre-made biological scaffolds for subsequent grafting of gelatin.
[0134] The procedure further includes a step (E) of manufacturing the PP64-gel scaffold into a biological scaffold for clinical application using a corresponding mold.
[0135] Example 7:
[0136] (A) PLLA and PLCL in a mass ratio of 7:3 were dissolved in 1,4-dioxane at 65°C to form a homogeneous polymer solution with a concentration of 10% (w / v);
[0137] (B) Pour into a preheated mold;
[0138] (C) Phase separation: The polymer solution and the mold were placed at -80°C for 24 hours and then freeze-dried for 72 hours to obtain the PP73 scaffold.
[0139] (D) Grafted gelatin: gelatin was fixed to the above PP73 scaffold using ammonolysis and glutaraldehyde (GA) crosslinking method to obtain PP73-gel scaffold.
[0140] In step (C), the PP73 scaffold can be a tubular scaffold or a circular scaffold, wherein the circular scaffold is fabricated in a steel mold (60 mm in diameter and 1 mm in height). Additionally, in step (C), thermally induced phase separation is used to prepare the biological scaffold preform.
[0141] In step (D), step (D) includes the following steps: (D1) removing impurities; (D2) aldehyde-based scaffold; and (D3) grafting gelatin. The specific operations of steps (D1)-(D3) are all as described in Example 1.
[0142] In step (A), a 10% w / v homogeneous polymer solution is formed.
[0143] The PP73 scaffolds obtained in steps (A), (B), and (C) are used as pre-made biological scaffolds for subsequent grafting of gelatin.
[0144] The procedure further includes a step (E) of manufacturing the PP73-gel scaffold into a biological scaffold for clinical application using a corresponding mold.
[0145] Example 8:
[0146] (A) PLLA and PLCL in a mass ratio of 8:2 were dissolved in 1,4-dioxane at 65°C to form a homogeneous polymer solution with a concentration of 10% (w / v);
[0147] (B) Pour into a preheated mold;
[0148] (C) Phase separation: The polymer solution and the mold were placed at -80°C for 24 hours and then freeze-dried for 72 hours to obtain the PP82 scaffold.
[0149] (D) Grafted gelatin: gelatin was fixed to the above PP82 scaffold by ammonolysis and glutaraldehyde (GA) crosslinking to obtain the PP82-gel scaffold.
[0150] In step (C), the PP82 scaffold can be a tubular scaffold or a circular scaffold, wherein the circular scaffold is fabricated in a steel mold (60 mm in diameter and 1 mm in height). Additionally, in step (C), thermally induced phase separation is used to prepare the biological scaffold preform.
[0151] In step (D), step (D) includes the following steps: (D1) removing impurities; (D2) aldehyde-based scaffold; and (D3) grafting gelatin. The specific operations of steps (D1)-(D3) are all as described in Example 1.
[0152] In step (A), a 10% w / v homogeneous polymer solution is formed.
[0153] The PP82 scaffolds obtained in steps (A), (B), and (C) are used as pre-made biological scaffolds for subsequent grafting of gelatin.
[0154] The procedure further includes a step (E) of manufacturing the PP82-gel scaffold into a biological scaffold for clinical application using a corresponding mold.
[0155] Example 9:
[0156] (A) PLLA and PLCL in a mass ratio of 9:1 were dissolved in 1,4-dioxane at 65°C to form a homogeneous polymer solution with a concentration of 10% (w / v).
[0157] (B) Pour into a preheated mold;
[0158] (C) Phase separation: The polymer solution and the mold were placed at -80°C for 24 hours and then freeze-dried for 72 hours to obtain the PP91 scaffold.
[0159] (D) Grafted gelatin: gelatin was fixed to the above PP91 scaffold by ammonolysis and glutaraldehyde (GA) crosslinking to obtain the PP91-gel scaffold.
[0160] In step (C), the PP91 scaffold can be a tubular scaffold or a circular scaffold, wherein the circular scaffold is fabricated in a steel mold (60 mm in diameter and 1 mm in height). Additionally, in step (C), thermally induced phase separation is used to prepare the biological scaffold preform.
[0161] In step (D), step (D) includes the following steps: (D1) removing impurities; (D2) aldehyde-based scaffold; and (D3) grafting gelatin. The specific operations of steps (D1)-(D3) are all as described in Example 1.
[0162] In step (A), a 10% w / v homogeneous polymer solution is formed.
[0163] The PP91 scaffolds obtained in steps (A), (B), and (C) are used as pre-made biological scaffolds for subsequent grafting of gelatin.
[0164] The procedure further includes a step (E) of manufacturing the PP91-gel scaffold into a biological scaffold for clinical application using a corresponding mold.
[0165] Those skilled in the art will understand that, through the methods described above in this invention, each embodiment can be supplemented with a step (E): manufacturing the grafted gelatin scaffold into a clinically applicable biological scaffold using a corresponding mold. It is understood that different molds can be used to manufacture different organ scaffolds, which can then be applied to the treatment of different organs. For example, the PP-gel scaffold can be manufactured using a ureteral scaffold mold, intestinal scaffold mold, esophageal scaffold mold, urethral scaffold mold, or vascular scaffold mold to obtain the clinically required ureteral scaffold, intestinal scaffold, esophageal scaffold, urethral scaffold, or vascular scaffold.
[0166] The characteristics of the pre-prepared biological scaffold and the grafted gelatin biological scaffold prepared in the above embodiments were tested.
[0167] 1. Porosity determination: The porosity of the scaffold was determined by the ethanol displacement method, because ethanol can enter the pores but will not cause the scaffold to shrink or expand.
[0168] 2. Observation of stent morphology: The morphology of the stent was observed using a scanning electron microscope (SEM: TM-3000, Hitachi).
[0169] 3. Determination of aperture and wall thickness: The aperture and wall thickness of the support were measured using Image-J software, with at least 50 measurements taken for each image.
[0170] 4. Contact angle determination: The hydrophilicity before and after gel coating was measured using a contact angle meter (datphysicsoca20, Germany). Before measurement, the sample was dried under vacuum at 30°C. After applying deionized water to the surface of the nanofiber scaffold for 10 seconds, the measurement was performed using software. For each sample, at least three independent measurements were performed and the average value was taken.
[0171] 5. Biocompatibility Study: Permanent human urine-derived cells (HUCs) were cultured in F12K medium (Gibco) containing 10% fetal bovine serum (FBS, Gibco), 100 U / ml penicillin, and 100 g / ml streptomycin (Gibco) at 37°C under humidification (5% CO2), with the medium being changed every two days. In the biocompatibility experiment, HUCs were placed on PP and PP-gel scaffolds. Cell proliferation on the scaffolds was detected using a Cell Counting Kit-8 (CCK-8). The distribution and morphology of cells on the scaffolds were observed using laser confocal microscopy (CLSM, SP8, Leica, Germany) and scanning electron microscopy (SEM).
[0172] 6. Cell viability and epithelialization detection: Cell cycle was detected by flow cytometry, epidermal growth factor was detected by EGF enzyme-linked immunosorbent assay kit, and epithelialization level was assessed by quantitative PCR.
[0173] 7. In vivo evaluation of tissue regeneration effect: Subcutaneous implantation was performed using 12 male SD rats, divided into two groups, for four and eight weeks of experimental use, respectively. The scaffolds were cut into circular sections, disinfected with 75% alcohol for 12 hours, and then implanted. After four and eight weeks, the scaffolds were removed, and H&E, Masson's immunohistochemistry (IHC), and immunofluorescence (IF) staining were used to analyze the scaffolds.
[0174] 8. Stent Biocompatibility Testing: CD68 assay was used to test the biocompatibility of the stent. Eighteen adult male New Zealand rabbits were divided into three groups for 8 and 12 weeks of treatment: the PP group, the PP-gel group, and the autologous ureter transplantation group. After anesthetizing the rabbits with pentobarbital (30 mg / kg), a midline abdominal incision was made. The left ureter was located along the paracolic gutter and the left ureteral defect (approximately 4 cm) was surgically removed. The graft was then placed at the ureteral defect site and sutured under a surgical microscope. A self-made ureteral stent was inserted into the ureter, and the stent was removed through the bladder incision two weeks post-operation. Histological observation was performed at 8 and 12 weeks post-operation.
[0175] 9. Epithelial cell detection: Epithelial cells were detected using AE1 / AE3, and the function of ureter after reconstruction in each group was analyzed using CT and CT urography (CTU).
[0176] The experimental results of the above embodiments are shown in the attached figures: Figure 2 The results of SEM analysis and determination of pore size and wall thickness of PP46 are shown, where a1 and a2 are the cross-sectional pore sizes, b1 and b2 are the cross-sectional wall thicknesses, and c1 and c2 are the surface pore sizes; (See attached image) Figure 3 The SEM analysis and pore size and wall thickness measurements of PP19 to PP91 and PP19-gel to PP91-gel prepared in the above nine embodiments are as follows: Figure 3Images A1-A9 show the SEM analysis and cross-sectional pore size determination results of the biological scaffold preforms PP19-PP91, while images a1-a9 show the SEM analysis and cross-sectional wall thickness determination results of PP19-gel-PP91-gel. (Attached) Figure 4 The porosity analysis results are shown for the bio-scaffold preform (PP scaffold) of the above embodiments. (Attached) Figure 5 The image shows the contact angle images and contact angle analysis charts for PP46 and PP46-gel stents. Figure 6 The stress curves of PP46 and PP46-gel are shown. Figure 7 The total reflectance infrared spectra of PP46 and PP46-gel with gelatin powder are shown. Figure 8 The results show the proliferation of epithelial cells. Figure 9 The results of subcutaneous implantation experiments in animals are shown. Figure 10 The image shown is of the stent after transplantation. Figure 11 The image shows the results of urothelialization detection. Figure 12 These are the results of a protein expression study.
[0177] This invention primarily focuses on PP46 and PP46-gel for research. Other proportions of biological scaffolds and biological scaffold preforms are validated and analyzed using the same method.
[0178] From the appendix Figure 2 To be continued Figure 4 It can be seen that the PP46 scaffold has a good internal pore structure, with an average pore diameter of 32.48±6.51μm (see attached). Figure 2 As shown in a1-a2), the cross-sectional wall thickness is 613.80±175.03nm (as shown in the attached diagram). Figure 2 As shown in Figures b1-b2, the surface of the PP46 support is also porous, with an average pore size of 3.74 ± 1.02 μm (as shown in the attached figure). Figure 2 (As shown in c1-c2).
[0179] Among all the stent ratios (PP19-PP91) in the above embodiments, electron microscopy observation of the internal pore structure shows that PP46 has the best internal structure and porosity, at 75.48±3.90% (see attached figure). Figure 4 As shown in the figure, the PP46 scaffold material has high porosity and large pores. This physical structure allows for cell migration and nutrient circulation, which is beneficial for promoting tissue regeneration.
[0180] like Figure 5 As shown, the contact angle of the PP46 stent is 98.50±2.93°, while that of the PP46-gel stent is 48.86±5.20°. This indicates that fixing gelatin to the stent significantly improves the hydrophilicity of the stent, giving the PP-gel stent higher hydrophilicity.
[0181] As attached Figure 6 The stress-strain curves of PP46 and PP46-gel scaffolds are shown. Due to ammonolysis, the tensile strength of the PP46-gel scaffold decreased (0.78±0.02 MPa vs 0.72±0.03 MPa, p<0.01), but the final strain did not change (84.62±3.09 MPa vs 84.88±3.22 MPa, p>0.05), indicating that the scaffold's toughness remained the same. This also shows that the toughness of PP46 and PP46-gel scaffolds is enhanced compared to polylactic acid, making them more suitable for tissue engineering applications.
[0182] The PP46 scaffold in this invention has optimal porosity and pore size, which not only facilitates nutrient circulation but also has anti-fibrotic effects. Furthermore, because the surface of the scaffold cools faster than the interior, a relatively dense porous structure can be formed on the scaffold surface, which is beneficial for epithelial formation while preventing cells from entering the scaffold.
[0183] Total reflectance infrared spectra of PP46 and PP46-gel with gelatin powder, as shown below Figure 7 As shown, the gelatinized scaffold has two characteristic absorption peaks of gelatin, while the PP46 scaffold does not, indicating that gelatin was successfully grafted onto the PP46 scaffold.
[0184] Repair of the urothelial layer is crucial for ureteral regeneration; therefore, the ability of urothelial cells to grow on scaffolds is an important question. HUS cells cultured on PP46 and PP46-gel scaffolds proliferated for seven days, with cultured polystyrene (TCPS) tissue cultured as a positive control.
[0185] Over time, HUS cells on both types of scaffolds continued to grow and proliferate, indicating that the scaffolds can support HUS proliferation without producing toxic effects. On day seven, the PP46-gel scaffold had more viable cells than the PP46 scaffold, indicating that the scaffold is more conducive to HUS proliferation after gelatin transplantation, as shown in the attached figure. Figure 8 As shown in A in the diagram.
[0186] Cell growth on a scaffold for three and seven days was observed using DAPI staining of the cytoskeleton and confocal microscopy. Figure 8 As shown in B, the cells on both scaffolds showed cytoskeleton disorder within three days. On the seventh day, the number of cells on both scaffolds increased, but the cytoskeleton on the PP46 scaffold remained disordered, while the cells on the PP46-gel scaffold had good morphology and expressed more actin bundles on the scaffold surface.
[0187] like Figure 8SEM analysis of C showed that hus grew on both scaffold surfaces and covered part of the pores on the scaffold surface. On the seventh day, cells were observed to cover more surface pores, especially on the PP46-gel scaffold.
[0188] like Figure 8 As shown in D, EGF is an important factor that promotes epithelialization. It can guide G0 phase cells back to G1 phase and carry out cell cycle proliferation. After seven days of culture, the GGF level in the PP46-gel group was significantly higher than that in the PP46 group, reaching 818.39±68.96 pg / ml.
[0189] like Figure 8 As shown in Figures E and F, the cell cycle distribution of urothelial cells was detected by flow cytometry. The cell proliferation index was calculated using the formula: proliferation index (%) = (S + G2 / M) / (G0 / G1 + S + G2 / M) x 100%. The proliferation index increased from (50.16 ± 2.25)% in the PP46 group to (56.04 ± 5.06)% in the PP46-gel group.
[0190] Animal experiments: PP46 and PP46-gel scaffolds were implanted subcutaneously into SD rats for 4 and 8 weeks, respectively. Figure 9 As shown in Figure A, the degree of vascularization on the scaffold surface increases over time. Compared with the two scaffolds used at the same time point, the PP46-gel scaffold exhibits a higher degree of vascularization. Vascularization of the outer layer of the scaffold is crucial for ureteral regeneration. HE and Masson staining revealed that once cells migrate to the scaffold surface, they secrete collagen, which promotes cell adhesion and proliferation. In gelatin-transplanted scaffolds, cells aggregate within the scaffold and secrete collagen. Furthermore, after 8 weeks, the gelatin scaffold shows significant degradation, allowing fibroblasts to pass through.
[0191] Inflammatory responses mainly occur in the early stages and are mostly expressed on the surface of the scaffold, such as... Figure 9 As shown in Figure B, semi-quantitative analysis revealed a significant decrease in inflammatory expression in the stent tissue cross-section at 8 weeks. Clinically, iatrogenic ureteral injury is the most common cause, especially in some typical surgical ureteroscopy procedures. The results of this experiment indicate that at 4 weeks, both types of stents showed positive signals on the surface and inside, with PP46 being higher than that of the PP46-gel stent, suggesting that the biocompatibility of the stents was improved after grafting gelatin. Figure 9 As shown in C, after 8 weeks, the number of positive models in the stent was significantly reduced, while the proportion of positive areas did not differ significantly.
[0192] Incomplete ureteral regeneration can cause ureteral dilation and hydronephrosis, thereby impairing kidney function. For example... Figure 10As shown, at 12 weeks post-operation, gross and CT / CTU images in the autologous transplant group revealed a certain degree of ureteral stenosis, but the degree of stenosis was lower in the PP46-gel group than in the PP46 group. The PP46 group exhibited significant ureteral and renal pelvis dilation and hydronephrosis, with no contrast enhancement of the left renal pelvis, indicating severe renal impairment. In the PP46-gel group, the degree of ureteral dilation was reduced and reversible. Figure 10 As shown in A in the diagram.
[0193] Hydronephrosis was observed using CT cross-sections, and the impact of the stent on renal function was assessed using Cr and BUN levels. After PP46-gel transplantation, the degree of hydronephrosis, Cr, and BUN decreased, indicating that the PP-gel group significantly reduced renal function impairment. Figure 10 As shown in BD.
[0194] Histological analysis was performed at 8 and 12 weeks postoperatively, and the results are as follows: Figure 10 As shown in Figure E. At 8 weeks, compared with the PP46-gel group, the PP46 group had more inflammatory cell infiltration, which disappeared at 12 weeks. Masson staining results showed that the PP46-gel scaffold degraded after two months, while the PP46 scaffold did not. In addition, normal collagen mechanisms replaced the scaffold in the PP46-gel group, while the PP46-gel group showed fibrosis due to excessive collagen proliferation, i.e., scar formation. Immunohistochemical staining of AE1 / AE was used to observe urothelial regeneration. After 8 weeks, the PP46 group showed a thinner layer of urothelial cells on the surface, while the PP46-gel group showed an increase in urothelial cells, and the number of cell layers increased over time. Therefore, the grafted gelatin scaffold promoted urothelialization, significantly reduced ureteral dilation and hydronephrosis, and protected renal function.
[0195] Three-dimensional ureteral engineering is a promising strategy for treating ureteral strictures, with one of its primary objectives being the formation of epithelial cells on the material surface. This study used immunofluorescence to detect the expression of urothelial cell-related functional proteins on two types of scaffolds. The results showed that the PP46-gel scaffold contained a higher concentration of cells, and these urothelial cells maintained an epithelial phenotype. Figure 11 As shown in A. ZO-1 and UPKIII are urothelial membrane proteins closely related to the role of urothelial obstruction of urine. RT-qPCR detection of the transcriptional levels of cell-related genes showed that the expression of membrane proteins such as UPK and ZO-1 was significantly increased, such as... Figure 11 As shown in B and C.
[0196] These results indicate that the grafted gelatin scaffold has the ability to promote urothelial proliferation, including the expression of genes related to cell proliferation and epithelial function. In addition, integrin α6, β4, K-RAS and N-RAS genes were also activated, demonstrating that the activation of the FAK / RAS-related pathway further promotes cell proliferation.
[0197] Figure 12 For protein expression studies, among which Figure 12 Figure A shows the expression of proteins from several pathways as detected by Western blotting. Consistent with the results of commercial RT-qPCR, the expression of p-FAK, integrin α6, β4, Ras, p-RAF, and p-ERK proteins was significantly increased in gelatin-modified scaffold cells. Figure 12 As shown in B in the diagram. Therefore, the PP46-gel scaffold can be shown to have a combined effect on the in vitro behavior and in vivo urothelialization of the urothelium, such as... Figure 12 As shown in C.
[0198] This indicates that integrin α6 / β4 senses the RGD sequence on the surface of the grafted gelatin scaffold, phosphorylating FAK and activating the downstream MAPK / ERK pathway. Furthermore, its internal porous structure provides more EGF to promote epithelial cell growth and proliferation. Urothelialization enables the formation of tight junctions between cells and AUM, thereby blocking the influence of urine on the submucosa. Therefore, the grafted gelatin PP porous scaffold has a role in promoting ureteral regeneration.
[0199] Those skilled in the art will understand that changing the ratio of PLL and PLCL can alter the pore size and wall thickness of the PP stent, or the ratio can be adjusted to other values to synthesize more PP stents, whose performance can then be studied to adapt to the stent requirements of different organs and meet more clinical applications.
[0200] In this invention, PP stents and PP-gel stents are used as ureteral stents to study their performance. The same or similar experimental methods can also be used to study them as biological stents for other organs to increase their clinical application scope.
[0201] The above research results show that the PP bioscaffold can be implanted in the ureter, which can significantly improve the healing of the urinary tract epithelium and delay the decline of renal function. The grafted gelatin scaffold can stimulate integrin α6 / β4 on the cell membrane of urinary tract epithelial cells, and then phosphorylate it under the action of focal adhesion kinase. It promotes epithelial formation through the mitogen-activated protein kinase / extracellular signal-regulated kinase signaling pathway. We found that the combined construction of biomimetic scaffold by nanomorphology and biochemistry can jointly stimulate ureteral regeneration.
[0202] In summary, this invention utilizes hexamethylenediamine ammonolysis and glutaraldehyde crosslinking to graft gelatin onto polyester, yielding various tubular porous PP-gel scaffolds. The PP46-gel scaffold, in particular, exhibits high hydrophilicity and good biocompatibility, promoting cell adhesion and proliferation, and facilitating ureteral epithelialization and regeneration, thus protecting ureteral and renal function. Therefore, the PP46-gel scaffold can serve as an ideal scaffold for constructing long segments of abnormal or defective ureters. Furthermore, with the development of tissue engineering, PP-gel scaffolds can also be used as scaffolds for other tissues and applied to the treatment of various organ diseases.
[0203] Those skilled in the art should understand that the embodiments of the present invention described above and shown in the accompanying drawings are merely examples and do not limit the present invention. The objectives of the present invention have been fully and effectively achieved. The functions and structural principles of the present invention have been demonstrated and explained in the embodiments, and any variations or modifications may be made to the implementation of the present invention without departing from the stated principles.
Claims
1. A method for preparing a gelatin-modified polylactic acid / polylactic acid-polycaprolactone copolymer, characterized in that, Includes the following steps: (A) A predetermined proportion of polylactic acid / polylactic acid-polycaprolactone copolymer is dissolved in 1,4-dioxane at 65°C to form a homogeneous polymer solution with a concentration of 10% (w / v), wherein the mass ratio of polylactic acid and polylactic acid-polycaprolactone copolymer is in the range of 1:9-9:
1. (B) The polymer solution is subjected to phase separation and freeze-drying. The difference in cooling rate between the surface and the interior of the support during the freezing process causes pores to be distributed in the polymer body, and the pores are more densely distributed on the surface of the polymer body than in the interior. The step (B) includes the following steps: (B1) pouring the polymer solution in step (A) into a preheated mold; (B2) performing phase separation by thermally induced phase separation. (B3) The polymer solution and mold were placed at -80°C for 24 hours, and then freeze-dried for 72 hours to obtain the polylactic acid / polylactic acid-polycaprolactone copolymer product; and (C) Grafted gelatin, wherein in this step, gelatin is fixed to the above polylactic acid / polylactic acid-polycaprolactone copolymer by ammonolysis and glutaraldehyde (GA) crosslinking to obtain gelatin-modified polylactic acid / polylactic acid-polycaprolactone copolymer product, wherein the ammonolysis treatment uses 1,6-hexanediamine as the ammonolysis reagent.
2. The method for preparing gelatin-modified polylactic acid / polylactic acid-polycaprolactone copolymer according to claim 1, wherein step (C) includes the following steps: (C1) The polylactic acid / polylactic acid-polycaprolactone copolymer product was soaked in 95% alcohol for 1 hour, then dried in a vacuum oven, and further soaked in 0.06 g / ml 1,6-hexanediamine / isopropanol solution for 10 minutes, and then rinsed with plenty of water to remove free hexanediamine, thereby obtaining a scaffold with impurities removed; (C2) The ammonolyzed polylactic acid / polylactic acid-polycaprolactone copolymer was soaked in 1.0 wt% GA aqueous solution at room temperature for 3 hours, and then rinsed with plenty of water to remove free GA, thereby obtaining an aldehyde-modified scaffold; (C3) The aldehyde-modified scaffold was cultured in 1.0 wt% gelatin / PBS solution at room temperature for 24 hours, and then the ungrafted gelatin was washed away with water to obtain gelatin-modified polylactic acid / polylactic acid-polycaprolactone copolymer.
3. The method for preparing gelatin-modified polylactic acid / polylactic acid-polycaprolactone copolymer according to claim 2, wherein... In step (A), the mass ratio of polylactic acid and polylactic acid-polycaprolactone copolymer is 1:9, 2:8, 3:7, 4:6, 5:5, 6:4, 7:3, 8:2 and 9:
1.
4. The gelatin-modified polylactic acid / polylactic acid-polycaprolactone copolymer prepared by the preparation method according to any one of claims 1 to 3, characterized in that, include: A polymer formed from polylactic acid and polylactic acid-polycaprolactone copolymer, wherein the polymer has at least one ester group suitable for decomposing an external group; as well as Gelatin, wherein the gelatin is grafted onto a product formed of polylactic acid and polylactic acid-polycaprolactone copolymer under predetermined conditions, wherein the mass ratio of polylactic acid to polylactic acid-polycaprolactone is 4:6.
Citation Information
Patent Citations
Preparation method of porous nano-fiber tubular scaffold
CN102908208A
Method for preparing gelatin surface graft modified polylactic acid microspheres
CN109172874A