A flotation collector for phosphorus minerals in polymetallic tailings and a preparation method and application thereof
By preparing a new flotation collector for phosphorus minerals in polymetallic tailings, and using components such as oxidized paraffin soap to improve water solubility and dispersibility, the problem of unsatisfactory flotation effect of phosphorus minerals in the existing technology was solved, and efficient recovery of phosphorus minerals was achieved.
Patent Information
- Application Number
- CN202410165510.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-05
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-02-05
AI Technical Summary
Existing flotation collectors for phosphate minerals are not effective and pollute the environment, making it difficult to efficiently separate useful phosphate minerals from tailings.
A collector prepared using oxidized paraffin soap, sodium oleate, starch, sodium dodecyl sulfonate, light tar oil, and sodium hydroxide improves flotation performance by enhancing water solubility and dispersibility, reducing surface tension of the slurry, increasing adsorption on the phosphate rock surface, promoting the formation of calcium oleate precipitate, and thus improving flotation efficiency.
This improved the flotation parameters of phosphate minerals, increased their grade and recovery rate, and enabled the efficient recovery of phosphate minerals from polymetallic tailings.
Smart Images

Figure CN117983410B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metallurgical and chemical technology, specifically relating to a flotation collector for phosphorus minerals in polymetallic tailings, its preparation method, and its application. Background Technology
[0002] Phosphate minerals are important industrial minerals, widely used in agriculture, food, and medicine. Because phosphate minerals exist primarily in complex mineral forms in nature, they require processing such as flotation to separate them. Currently available phosphate mineral flotation collectors suffer from unsatisfactory performance and environmental pollution. Therefore, developing and selecting a novel phosphate mineral flotation collector and its preparation method is of great significance, especially for separating useful phosphate minerals from tailings. Summary of the Invention
[0003] The first objective of this invention is to provide a flotation collector for phosphorus minerals in polymetallic tailings; the second objective is to provide a method for preparing the aforementioned flotation collector for phosphorus minerals in polymetallic tailings; and the third objective is to provide an application of the aforementioned flotation collector for phosphorus minerals in polymetallic tailings.
[0004] The first objective of this invention is achieved as follows: the flotation collector for phosphorus minerals in polymetallic tailings is composed of 10-30 parts by weight of oxidized paraffin soap, 5-20 parts by weight of sodium oleate, 10-30 parts by weight of starch, 2-8 parts by weight of sodium dodecyl sulfonate, 5-20 parts by weight of light tar oil, and 2-8 parts by weight of sodium hydroxide.
[0005] The second objective of this invention is achieved by including pretreatment and preparation steps, specifically including: A. Pre-processing: 1) Add distilled water to the sodium hydroxide solution in the formula and stir to dissolve it to obtain alkaline solution a; 2) Mix the oxidized paraffin soap, sodium oleate and sodium dodecyl sulfonate according to the formula, add distilled water and stir to obtain mixture b; B. Preparation: 1) Add the starch according to the formula to alkaline solution a and stir evenly to obtain mixture c; 2) Add mixture b to mixture c and stir to obtain mixture d; 3) Add the light tar oil of the formula to the mixture d and stir evenly to obtain the flotation collector for phosphorus minerals in polymetallic tailings.
[0006] The third objective of this invention is achieved by the application of the phosphorus mineral flotation collector in the flotation process of phosphorus-containing polymetallic tailings.
[0007] This invention relates to a collector prepared from oxidized paraffin soap, sodium oleate, starch, sodium dodecyl sulfonate, light tar oil, sodium hydroxide, and water. This collector possesses good collecting, foaming, and conditioning abilities, improving the water solubility and dispersibility of oxidized paraffin soap and sodium oleate in slurry, reducing the surface tension of the slurry and the Zeta potential of the phosphate rock, increasing the adsorption capacity of the collector on the phosphate rock surface, and promoting the reaction of hydrolyzed oleate ions with CaO on the phosphate rock surface. 2+ The reaction produces calcium oleate precipitate, thereby improving the flotation effect of phosphate rock and increasing flotation index. Attached Figure Description
[0008] Figure 1 This is a schematic diagram of the process flow of the present invention. Detailed Implementation
[0009] The present invention will be further described below with reference to embodiments, but this is not intended to limit the present invention in any way. Any modifications or substitutions made based on the teachings of the present invention shall fall within the protection scope of the present invention.
[0010] The flotation collector for phosphorus minerals in polymetallic tailings described in this invention is composed of 10-30 parts by weight of oxidized paraffin soap, 5-20 parts by weight of sodium oleate, 10-30 parts by weight of starch, 2-8 parts by weight of sodium dodecyl sulfonate, 5-20 parts by weight of light tar oil, and 2-8 parts by weight of sodium hydroxide.
[0011] The flotation collector for phosphorus minerals in polymetallic tailings is composed of 16-26 parts by weight of oxidized paraffin soap, 8-16 parts by weight of sodium oleate, 15-25 parts by weight of starch, 3-5 parts by weight of sodium dodecyl sulfonate, 8-14 parts by weight of light tar oil, and 3-7 parts by weight of sodium hydroxide.
[0012] The flotation collector for phosphorus minerals in polymetallic tailings is composed of 21 parts by weight of oxidized paraffin soap, 12 parts of sodium oleate, 20 parts of starch, 4 parts of sodium dodecyl sulfonate, 11 parts of light tar oil, and 5 parts of sodium hydroxide.
[0013] The preparation method of the flotation collector for phosphorus minerals in polymetallic tailings according to the present invention includes pretreatment and formulation steps, specifically including: A. Pre-processing: 1) Add distilled water to the sodium hydroxide solution in the formula and stir to dissolve it to obtain alkaline solution a; 2) Mix the oxidized paraffin soap, sodium oleate and sodium dodecyl sulfonate according to the formula, add distilled water and stir to obtain mixture b; B. Preparation: 1) Add the starch according to the formula to alkaline solution a and stir evenly to obtain mixture c; 2) Add mixture b to mixture c and stir to obtain mixture d; 3) Add the light tar oil of the formula to the mixture d and stir evenly to obtain the flotation collector for phosphorus minerals in polymetallic tailings.
[0014] The application of this invention is the use of the phosphorus mineral flotation collector in the flotation process of phosphorus-containing polymetallic tailings.
[0015] The invention will be further illustrated below with specific implementation examples: Example 1
[0016] 1) Add 20g of sodium hydroxide to distilled water and stir to dissolve to obtain alkaline solution a; 2) Mix 100g of oxidized paraffin soap, 50g of sodium oleate, and 20g of sodium dodecyl sulfonate, then add distilled water and stir to obtain mixture b; B. Preparation: 1) Add 100g of starch to alkaline solution a and stir until well mixed to obtain mixture c; 2) Add mixture b to mixture c and stir to obtain mixture d; 3) Add 50g of light tar oil to the mixture d and stir evenly to obtain the flotation collector for phosphorus minerals in polymetallic tailings.
[0017] Example 2
[0018] 1) Dissolve 80g of sodium hydroxide in distilled water by stirring to obtain alkaline solution a; 2) Mix 300g of oxidized paraffin soap, 200g of sodium oleate and 80g of sodium dodecyl sulfonate, then add distilled water and stir to obtain mixture b; B. Preparation: 1) Add 300g of starch to alkaline solution a and stir until homogeneous to obtain mixture c; 2) Add mixture b to mixture c and stir to obtain mixture d; 3) Add 200g of light tar oil to the mixture d and stir evenly to obtain the flotation collector for phosphorus minerals in polymetallic tailings.
[0019] Example 3
[0020] 1) Add 50g of sodium hydroxide to distilled water and stir to dissolve to obtain alkaline solution a; 2) Mix 210g of oxidized paraffin soap, 120g of sodium oleate and 40g of sodium dodecyl sulfonate, then add distilled water and stir to obtain mixture b; B. Preparation: 1) Add 200g of starch to alkaline solution a and stir until well mixed to obtain mixture c; 2) Add mixture b to mixture c and stir to obtain mixture d; 3) Add 110g of light tar oil to the mixture d and stir evenly to obtain the flotation collector for phosphorus minerals in polymetallic tailings.
[0021] Example 4
[0022] 1) Dissolve 60g of sodium hydroxide in distilled water by stirring to obtain alkaline solution a; 2) Mix 200g of oxidized paraffin soap, 150g of sodium oleate and 60g of sodium dodecyl sulfonate, then add distilled water and stir to obtain mixture b; B. Preparation: 1) Add 150g of starch to alkaline solution a and stir until well mixed to obtain mixture c; 2) Add mixture b to mixture c and stir to obtain mixture d; 3) Add 150g of light tar oil to the mixture d and stir evenly to obtain the flotation collector for phosphorus minerals in polymetallic tailings.
[0023] Example 5
[0024] 1) Add 50g of sodium hydroxide to distilled water and stir to dissolve to obtain alkaline solution a; 2) Mix 130g of oxidized paraffin soap, 120g of sodium oleate and 70g of sodium dodecyl sulfonate, then add distilled water and stir to obtain mixture b; B. Preparation: 1) Add 180g of starch to alkaline solution a and stir until well mixed to obtain mixture c; 2) Add mixture b to mixture c and stir to obtain mixture d; 3) Add 130g of light tar oil to the mixture d and stir evenly to obtain the flotation collector for phosphorus minerals in polymetallic tailings.
[0025] Example 6
[0026] The flotation collector for phosphorus minerals in polymetallic tailings prepared in Example 3 was used in the experiment, as follows: 1) A multi-element chemical analysis was performed on a polymetallic ore from Hebei Province, and the results are shown in Table 1. A phosphorus phase analysis was performed on the tailings, and the results are shown in Table 2.
[0027] Table 1. Multi-element chemical analysis of the raw ore Table 2. Phase analysis of phosphorus in tailings The main recoverable valuable metallic elements in the raw ore are iron, vanadium, titanium, and copper, while the main valuable non-metallic element is phosphorus. Phosphorus phase analysis of the polymetallic tailings shows that phosphorus mainly exists in the form of apatite. The closed-circuit process test for phosphorus beneficiation adopts a process flow of one roughing, two cleaning, and one scavenging, as follows: Figure 1 As shown in the figure. The roughing depressant was 80 g / t of water glass, and the flotation collector for phosphorus minerals in the polymetallic tailings prepared in Example 3 was 200 g / t. The primary cleaning depressant was 40 g / t, the secondary cleaning depressant was 20 g / t, and the flotation collector for phosphorus minerals in the polymetallic tailings prepared in Example 3 was 100 g / t. A phosphorus concentrate with a grade of 30.13% and a recovery rate of 92.22% was finally obtained, achieving efficient recovery of low-grade phosphorus minerals from polymetallic tailings.
[0028] 2) A multi-element chemical analysis was performed on a polymetallic ore in Liaoning Province. The results are shown in Table 3.
[0029] Table 3 Chemical composition and content of raw ore Table 3 shows that Fe, TiO2, MgO, and P2O5 are the components with recovery value in the raw ore. The closed-circuit process test for phosphorus beneficiation adopted a process flow of one roughing, two cleaning, and one scavenging, as follows: Figure 1 As shown. The roughing depressant was 60 g / t of water glass, and the flotation collector for phosphorus minerals in the polymetallic tailings prepared in Example 3 was 400 g / t. The primary cleaning depressant was 30 g / t, the secondary cleaning depressant was 15 g / t, and the flotation collector for phosphorus minerals in the polymetallic tailings prepared in Example 3 was 200 g / t. A phosphorus concentrate with a grade of 38.29% and a recovery rate of 85.68% was finally obtained, achieving the flotation recovery and utilization of low-grade phosphorus minerals in polymetallic tailings.
[0030] Example 7
[0031] The flotation collectors for phosphorus minerals in polymetallic tailings prepared in Examples 1, 2, 4 and 5 were tested respectively. The results showed that the flotation collectors for phosphorus minerals in polymetallic tailings described in this invention can increase the grade by 1% to 3% and the recovery rate by 4% to 6% compared with the same period last year.
Claims
1. A flotation collector for phosphorus minerals in polymetallic tailings, characterized in that, The collector is composed of the following raw materials in parts by weight: 21 parts of oxidized paraffin soap, 12 parts of sodium oleate, 20 parts of starch, 4 parts of sodium dodecyl sulfonate, 11 parts of light tar oil, and 5 parts of sodium hydroxide. The method for preparing the collector includes the following steps: A. Pre-processing: 1) Add the specified amount of sodium hydroxide to distilled water and stir to dissolve, to obtain alkaline solution a; 2) Mix the specified weight parts of oxidized paraffin soap, sodium oleate and sodium dodecyl sulfonate, then add distilled water and stir to mix well to obtain mixture b; B. Preparation: 1) Add the starch by weight to alkaline solution a and stir until homogeneous to obtain mixture c; 2) Add mixture b to mixture c and stir to obtain mixture d; 3) Add the specified weight of light tar oil to the mixture d and stir evenly to obtain the target product, the phosphorus mineral flotation collector in polymetallic tailings; The phosphorus mineral flotation collector in the polymetallic tailings is applied to the flotation process of phosphorus-containing polymetallic tailings.
Citation Information
Patent Citations
Beneficiation method of polymetallic ore cassiterite