A method for preparing high-performance nickel-based superalloy / ceramic composite materials by laser powder bed fusion technology
By mixing SiC ceramic powder with IN718 high-temperature alloy powder and using laser powder bed melting technology, the forming defects and mechanical properties of nickel-based high-temperature alloy/ceramic composite materials were solved, and the preparation of high-performance composite materials was realized.
Patent Information
- Application Number
- CN202410197655.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-22
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-02-22
AI Technical Summary
Existing laser powder bed melting technology has problems such as numerous forming defects, poor mechanical properties, and the introduction of foreign alloying elements when preparing nickel-based superalloy/ceramic composite materials.
High-performance nickel-based high-temperature alloy/ceramic composite materials were prepared by mixing SiC ceramic powder with IN718 high-temperature alloy powder, followed by uniform mixing through ball milling and ultrasonic vibration, and then laser powder bed melting and forming. The laser parameters and protective gas were controlled.
It significantly refines the grains, improves the strength and hardness of the composite material, reduces forming defects, and enhances molding quality and mechanical properties.
Smart Images

Figure CN117983834B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of laser additive manufacturing technology, and specifically to a method for preparing high-performance nickel-based superalloy / ceramic composite materials using laser powder bed melting technology. Background Technology
[0002] With the rapid development of aero-engine technology, improving the thrust-to-weight ratio, enhancing structural reliability and durability, and reducing fuel consumption have become key technologies for improving engine performance. Nickel-based superalloys possess excellent oxidation and hot corrosion resistance, superior fatigue resistance, high structural stability, and high reliability, making them widely used in critical hot-end components in aerospace, nuclear industry, energy and power, and petrochemical fields. They are irreplaceable key materials for modern national defense and economic development. IN718 is a precipitation-strengthened nickel-based superalloy with the highest yield strength among wrought superalloys below 650℃. It exhibits good fatigue resistance, radiation resistance, and high-temperature stability, and is widely used in fans, casings, turbine disks, fasteners, and connecting bearings. Currently, IN718 superalloy has become the most produced and widely used superalloy in the aerospace industry, accounting for more than 35% of the total superalloy production. SiC ceramics, due to their high tensile strength, relatively stable high-temperature properties, and operating temperature up to 1200℃, have become a particulate reinforcement material for metals and ceramics. Adding ceramic particles to nickel-based superalloys not only increases the service temperature of the composite material (600-1000℃) but also improves its service performance, which has become a research focus in recent years.
[0003] Laser powder bed melting (LPM) technology utilizes a high-energy laser beam to scan and melt thin layers of powder layer by layer. It offers advantages such as high forming accuracy, short processing cycles, and no need for subsequent processing. This technology breaks through the constraints and limitations of traditional manufacturing forming techniques and structural design, providing new research ideas for the development of complex structural components and meeting the rapidly evolving needs of forming technologies in fields such as aerospace. However, the rapid cooling rate and high temperature gradient generated during laser rapid prototyping result in a significantly finer grain structure compared to traditional casting, leading to anisotropic mechanical properties and affecting service life. Table 1 summarizes the classification, preparation methods, and costs of different nickel-based superalloy / ceramic composite materials.
[0004] Table 1. Comparison of different nickel-based superalloy / ceramic composite materials in terms of classification, preparation methods, and costs.
[0005]
[0006] Chinese patent CN112522564A relates to a method for preparing TiB2 particle-reinforced nickel-based superalloys. First, a nickel-based superalloy (IN718) is melted under high temperature and vacuum. TiB2 is then added to the molten alloy, followed by heat preservation and casting. This method significantly reduces dendrite spacing, refines the grains, and improves the strength of the composite material. However, this method is complex, suffers from microscopic segregation between dendrites, and cannot determine whether TiB2 is uniformly added to the molten alloy.
[0007] Chinese patent CN116604031A relates to a method for improving the hardness of IN718 alloy produced by laser additive manufacturing. Al is added to IN718 high-temperature alloy powder by powder ball milling to increase the hardness of the alloy. However, excessive Al promotes the segregation of Nb, resulting in the precipitation of a large number of brittle LAVEs with continuous chain and network distribution in the microstructure, without addressing the issues of microstructure homogenization and strength.
[0008] The literature “D Gu, H Zhang, D Dai, et al. Laser additive manufacturing of nano-TiC reinforced Ni-based nanocomposites with tailored microstructure and performance. Composites Part B Engineering, 2019, 163: 585-597” uses laser powder bed melting to prepare IN718 / TiC composite materials. However, the formed samples contain many small pores, which reduce the density, decrease the molding quality, and hinder the improvement of mechanical properties.
[0009] The literature "I Ho,T Hsu,Y Chang,et.al.Effects of CoAl2O4 inoculants on microstructure and mechanical properties of IN718 processed by selective laser melting.Additive Manufacturing,2020,35:101328" describes the addition of 0.2wt% CoAl2O4 powder to the original IN718 high-temperature alloy powder via ball milling, followed by laser powder bed melting to form a composite powder. This improved the residual stress in the deposited state and enhanced the mechanical properties, but introduced a metallic element other than the alloying elements, which could not be removed subsequently.
[0010] To optimize the quality of laser powder bed fusion-formed composite materials, reduce forming defects, and further improve mechanical properties, ceramic particles are added to high-temperature alloys. The size, introduction method, physicochemical properties, and interfacial compatibility of the ceramic particles determine the forming quality. Furthermore, the composition, shape, and size of the composite powder, laser rapid prototyping parameters, and forming environment are all closely related to forming accuracy. The microstructure grain size needs further refinement, and strength and hardness need improvement. Therefore, powder preparation and ceramic particle selection are crucial for the formation of high-performance composite materials using laser powder bed fusion-formed materials. Summary of the Invention
[0011] The purpose of this invention is to provide a method for preparing high-performance nickel-based superalloy / ceramic composite materials using laser powder bed melting technology. The preparation method provided by this invention can refine grains, improve strength and hardness, and enhance the overall performance of nickel-based superalloy / ceramic composite materials.
[0012] To achieve the above-mentioned objectives, the present invention provides the following technical solution:
[0013] This invention provides a method for preparing high-performance nickel-based superalloy / ceramic composite materials using laser powder bed melting technology, comprising the following steps:
[0014] Ceramic powder and nickel-based high-temperature alloy powder are mixed to obtain a mixed powder;
[0015] The mixed powder is subjected to laser powder bed melting to obtain a high-performance nickel-based high-temperature alloy / ceramic composite material.
[0016] Preferably, the ceramic powder is SiC powder; the nickel-based high-temperature alloy powder is IN718 high-temperature alloy powder.
[0017] Preferably, the mass ratio of the ceramic powder to the nickel-based high-temperature alloy powder is 0.001 to 0.1:1.
[0018] Preferably, the size of the ceramic powder is 0.001 to 200 μm; the particle size of the nickel-based high-temperature alloy powder is 15 to 53 μm.
[0019] Preferably, the mixing of the ceramic powder and the nickel-based superalloy powder includes sequential ball milling and ultrasonic vibration.
[0020] Preferably, the ball milling is a wet ball milling; the rotation speed of the ball mill is 100-500 r / min; and the ball milling time is 2-12 h.
[0021] Preferably, the power of the ultrasonic vibration is 50-80W, and the duration of the ultrasonic vibration is 0.5-4h.
[0022] Preferably, the conditions for laser powder bed melting and forming include: laser power of 100-500W, scanning rate of 300-2000mm / s, scanning spacing of 30-90μm, processing layer thickness of 30-60μm, and spot diameter of 75μm.
[0023] Preferably, the laser scanning method for the laser powder bed melting and forming is one of X, Y, and XY.
[0024] Preferably, the protective gas used during the laser powder bed melting and forming process is high-purity argon; the oxygen content of the high-purity argon is less than 1000 ppm.
[0025] This invention provides a method for preparing high-performance nickel-based superalloy / ceramic composite materials using laser powder bed melting technology. Compared with existing methods for preparing nickel-based superalloy / ceramic composite materials, this method is convenient, simple, highly universal, produces materials with excellent properties, and can form components of any complex shape.
[0026] As a preferred embodiment, the present invention has the following advantages:
[0027] (1) In this invention, SiC ceramic particles are added to a nickel-based superalloy to form a composite material. The addition of SiC does not introduce other alloying elements, avoiding cumbersome removal processes. SiC has a high melting point (2827℃) and does not easily react with the alloy melt. At high temperatures, SiC decomposes into Si ions and C ions. When free silicon ions are present, Nb and Ti tend to form silicides, and MC carbides nucleate around Al2O3 particles, pinning grain boundaries and increasing grain boundary strength.
[0028] (2) The mixed powder preparation process provided by this invention is simple. SiC powder and IN718 high-temperature alloy powder are mixed using anhydrous ethanol as a dispersant and binder through low-speed ball milling. Appropriate ultrasonic vibration and stirring further ensure a more uniform mixture, guaranteeing that SiC is uniformly adhered to the surface of the IN718 alloy spherical particles. During subsequent drying, SiC and IN718 maintain good bonding, which is beneficial for the spreading of the laser powder bed. Furthermore, the presence of SiC ceramic particles refines the microstructure, reducing the grain size from 17.54 μm to 14.37 μm, thus reducing stress concentration and improving mechanical properties.
[0029] (3) The method for preparing high-performance nickel-based superalloy / ceramic composite materials provided by this invention is simple, effectively reduces solidification defects in the forming process, improves the forming quality of the deposited state, saves manufacturing costs of superalloy / ceramic composite materials, reduces post-processing costs, and has wide applicability. This method provides a new technical approach for the preparation of nickel-based superalloy / ceramic composite materials and has good application prospects in the aerospace field. Attached Figure Description
[0030] Figure 1 This is a process flow diagram for preparing the high-performance nickel-based superalloy / ceramic composite material of the present invention;
[0031] Figure 2 The images show the microstructure and particle size distribution of the dried mixed powder and IN718 high-temperature alloy powder prepared in Examples 1, 2 and Comparative Example 1 of this invention.
[0032] Figure 3 IN718 / SiC prepared according to Example 1 of the present invention and with different laser powers μm Sample image of the composite material;
[0033] Figure 4 IN718 / SiC prepared in Example 1 of this invention μm Microstructure of the composite material;
[0034] Figure 5 IN718 / SiC prepared in Example 2 of this invention nm Microstructure of the composite material;
[0035] Figure 6 The image shows the microstructure of the IN718 high-temperature alloy prepared in Comparative Example 1 of this invention.
[0036] Figure 7 Comparison of room temperature tensile curves of the high-performance nickel-based superalloy / ceramic composite material and IN718 superalloy prepared in Examples 1 and 2 of the present invention and Comparative Example 1;
[0037] Figure 8 This is a comparison of the microhardness of the high-performance nickel-based superalloy / ceramic composite material and IN718 superalloy prepared by changing the laser power of Examples 1, 2 and Comparative Example 1 according to the present invention. Detailed Implementation
[0038] This invention provides a method for preparing high-performance nickel-based superalloy / ceramic composite materials using laser powder bed melting technology, comprising the following steps:
[0039] Ceramic powder and nickel-based high-temperature alloy powder are mixed to obtain a mixed powder;
[0040] The mixed powder is subjected to laser powder bed melting to obtain a high-performance nickel-based high-temperature alloy / ceramic composite material.
[0041] This invention mixes ceramic powder and nickel-based superalloy powder to obtain a mixed powder. In this invention, the ceramic powder is preferably SiC powder; the nickel-based superalloy powder is preferably IN718 superalloy powder. In this invention, the size of the ceramic powder is preferably 0.001–200 μm, more preferably 0.001–100 μm. In this invention, when the ceramic powder is spherical, the particle size range is preferably 15–53 μm, more preferably 20–30 μm; when the ceramic powder is irregularly shaped, the particle size range is preferably 0.63–1.03 μm, more preferably 0.75–0.85 μm. In this invention, the particle size range of the nickel-based superalloy powder is preferably 15–53 μm, more preferably 20–30 μm. This invention, by controlling the ceramic powder of different sizes, obtains a nickel-based superalloy / ceramic composite material with good formability and excellent mechanical properties.
[0042] In this invention, the mass ratio of the ceramic powder to the nickel-based high-temperature alloy powder is preferably 0.001 to 0.1:1, more preferably 0.02 to 0.05:1.
[0043] In this invention, the mixing of the ceramic powder and the nickel-based high-temperature alloy powder preferably includes sequential ball milling and ultrasonic vibration. In this invention, the ball milling is preferably wet ball milling; the medium for the wet ball milling is preferably anhydrous ethanol. In this invention, the rotation speed of the ball mill is preferably 100–500 r / min, more preferably 200–300 r / min; the rotation direction of the ball mill is preferably 360°; the ball milling time is preferably 2–12 h, more preferably 4–8 h. In this invention, the grinding balls used in the ball mill are preferably made of 304 stainless steel, and the ball-to-material mass ratio is preferably 2–3:1.
[0044] In this invention, the power of the ultrasonic vibration is preferably 50-80W, more preferably 65-70W; the duration of the ultrasonic vibration is preferably 0.5-4h, more preferably 2-3h. This invention uses ball milling and ultrasonic vibration to uniformly adhere ceramic powder to the surface of nickel-based high-temperature alloy powder.
[0045] In this invention, the ceramic powder and nickel-based high-temperature alloy powder are mixed, and then the resulting material is dried to obtain a mixed powder. This invention removes moisture through drying. In this invention, the drying temperature is preferably 50–100°C, more preferably 80–90°C; the drying time is preferably 4–24 hours, more preferably 8–12 hours. In this invention, the drying is preferably carried out in a vacuum drying oven or an electrically heated forced-air drying oven.
[0046] Preferably, the mixture is sieved after drying to obtain a mixed powder. In this invention, the particle size of the mixed powder is preferably 15–55 μm, more preferably 20–30 μm.
[0047] After obtaining the mixed powder, the present invention performs laser powder bed melting to obtain a high-performance nickel-based high-temperature alloy / ceramic composite material. In the present invention, the preferred conditions for laser powder bed melting include: laser power of 100–500 W, scanning rate of 300–2000 mm / s, scanning spacing of 30–90 μm, processed layer thickness of 30–60 μm, and spot diameter of 75 μm. In the present invention, the laser power is more preferably 200–300 W; the scanning rate is more preferably 833–1000 mm / s; the scanning spacing is more preferably 75–80 μm; and the processed layer thickness is more preferably 40–50 μm. In the present invention, the laser scanning mode for laser powder bed melting is preferably one of X, Y, and XY, more preferably XY.
[0048] In this invention, the protective gas used during the laser powder bed melting process is preferably high-purity argon. Preferably, the purity of the high-purity argon is greater than 99.99 wt.%; the oxygen content of the high-purity argon is preferably less than 1000 ppm, more preferably less than 500 ppm, and even more preferably less than 300 ppm. By performing laser powder bed melting under the aforementioned protective atmosphere, this invention can prevent oxygen from reacting with the mixed powder.
[0049] In a specific embodiment of the present invention, based on the characteristics of laser powder bed melting forming, the model is designed on a computer using 3D modeling software, saved in STL format, and imported into the professional ARPS software of the laser powder bed melting forming equipment for layering and slicing, and path planning is performed.
[0050] In a specific embodiment of the present invention, 304 stainless steel is selected as the substrate; during the laser powder bed melting process, the substrate is preheated to 100°C.
[0051] In a specific embodiment of the present invention, the preparation process of the high-performance nickel-based superalloy / ceramic composite material is as follows: Figure 1 As shown.
[0052] The technical solutions of this invention will be clearly and completely described below with reference to the embodiments thereof. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0053] The specific composition of the IN718 high-temperature alloy powder used in the examples and comparative examples is as follows: Cr: 19.14wt%, Mo: 3.13wt%, Nb: 5.41wt%, Fe: 18.63wt%, Co: 0.28wt%, Ti: 0.76wt%, Al: 0.23wt%, Si: 0.18wt%, C: 0.019wt%, Mn: 0.044wt%, Cu: 0.028wt%, Ni: Bal.
[0054] Example 1
[0055] A method for preparing high-performance nickel-based superalloy / ceramic composite materials using laser powder bed melting technology, comprising the following specific steps:
[0056] Spherical SiC powder (SiC μm The SiC powder and IN718 high-temperature alloy powder were placed in the grinding jar of a planetary ball mill, and anhydrous ethanol (purity 99.5 wt.%) was added to completely submerge the powder. The particle size distribution of the spherical SiC powder was 15–53 μm, and the particle size distribution of the IN718 high-temperature alloy powder was also 15–53 μm. The mass of the spherical SiC powder was 2.0% of the total mass of the spherical SiC powder and IN718 high-temperature alloy powder. The grinding balls were made of 304 stainless steel, and the ball-to-powder mass ratio was controlled at 2:1. The rotation direction was 360°, the rotation speed was 200 r / min, and the grinding time was 8 h. After ball milling, the resulting ball-milled system was subjected to ultrasonic vibration in an ultrasonic cleaner. The ultrasonic vibration power was 65 W, each session lasted 30 min, and the process was repeated 4 times with a 10 min interval between each session. The ultrasonically treated product was placed in a forced-air drying oven at 80°C for 12 hours, and then sieved to obtain a dried mixed powder with a particle size of 15–55 μm.
[0057] Based on the characteristics of laser powder bed fusion forming, a model was designed on a computer using 3D modeling software, saved as an STL file, and imported into the professional ARPS software of the laser powder bed fusion forming equipment for layering and slicing, and path planning. 304 stainless steel was selected as the substrate. During the laser powder bed fusion forming process, the substrate was preheated to 100℃, and 99.99wt.% high-purity argon gas was introduced as a protective gas, with an oxygen content below 300ppm.
[0058] The laser powder bed melting process parameters were set as follows: laser power of 250W, scanning rate of 833mm / s, processing layer thickness of 50μm, scanning spacing of 75μm, laser scanning mode of XY, and spot diameter of 75μm. The dried mixed powder prepared above was then subjected to laser powder bed melting to obtain IN718 / SiC. μm Composite material (IN718+2% SiC)μm -250W). Then, each IN718 / SiC element was cut using wire EDM. μm The composite material was cut from a 304 stainless steel substrate.
[0059] Figure 2 Images (a1) and (a2) are scanning electron microscope (SEM) images of the dried mixed powder described in Example 1 of this invention. Figure 2 (a3) is the particle size distribution diagram of the dried mixed powder described in Example 1; Figure 2 (c1) and (c2) are scanning electron microscope images of IN718 high-temperature alloy powder. Figure 2 (c3) is the particle size distribution diagram of IN718 high-temperature alloy powder. It can be seen from the figure that SiC... μm SiC is uniformly mixed with IN718 high-temperature alloy powder. μm The addition of [a substance] increases the average particle size of IN718 high-temperature alloy powder.
[0060] Figure 3 IN718 / SiC prepared according to Example 1 of the present invention and with different laser powers μm A sample image of the composite material.
[0061] Figure 4 IN718 / SiC prepared in Example 1 of this invention μm Microstructure of the composite material. SiC μm The addition of SiC significantly refined the grain size. μm During laser powder bed melting, decomposition occurs, breaking down into free Si and C ions. In the presence of free silicon ions, Nb and Ti tend to form silicides; MC carbides nucleate and grow around Al2O3 particles.
[0062] The room temperature yield strength, tensile strength, and elongation were tested according to GB / T 32498-2016, and the microhardness was tested according to GB / T 9790-2021. IN718 / SiC prepared in Example 1... μm The composite material has a room temperature yield strength of 774 MPa, a tensile strength of 1016 MPa, an elongation of 13%, and a microhardness of 355 HV.
[0063] Example 2
[0064] Irregularly shaped SiC powder (SiC nmThe SiC powder and IN718 high-temperature alloy powder were placed in the grinding jar of a planetary ball mill, and anhydrous ethanol (purity 99.5 wt.%) was added to completely submerge the powder. The irregularly shaped SiC powder had a particle size distribution of 0.63–1.03 μm, and the IN718 high-temperature alloy powder had a particle size distribution of 15–53 μm. The mass of the irregularly shaped SiC powder was 2.0% of the total mass of the irregularly shaped SiC powder and IN718 high-temperature alloy powder. The grinding balls were made of 304 stainless steel, with a ball-to-powder mass ratio of 3:1, a rotation direction of 360°, a rotation speed of 300 r / min, and a grinding time of 4 hours. After grinding, the resulting ball-milled system was subjected to ultrasonic vibration in an ultrasonic cleaner with a power of 65 W, for 30 minutes each time, for 4 times, with a 10-minute interval between each vibration. The ultrasonically treated product was placed in a forced-air drying oven at 80°C for 12 hours, and then sieved to obtain a dried mixed powder with a particle size of 15–55 μm.
[0065] The dried mixed powder was subjected to laser powder bed melting to obtain IN718 / SiC. nm Composite material (IN718+2% SiC) nm -250W); The process and parameters of laser powder bed melting are the same as in Example 1.
[0066] Figure 2 Images (b1) and (b2) are scanning electron microscope (SEM) images of the dried mixed powder described in Example 2 of this invention. Figure 2 Figure (b3) shows the particle size distribution of the dried mixed powder described in Example 2. As can be seen from the figure, SiC... nm SiC is uniformly adhered to the surface of IN718 high-temperature alloy powder. nm The addition of [a substance] increases the average particle size of IN718 high-temperature alloy powder.
[0067] Figure 5 IN718 / SiC prepared in Example 2 of this invention nm Microstructure of the composite material.
[0068] SiC nm The addition of [a specific ingredient] significantly refined the grain structure of the IN718 high-temperature alloy, resulting in the presence of more silicides and [other components].
[0069] MC carbides.
[0070] Using the same testing methods as in Example 1, the IN718 / SiC prepared in Example 2... nm The composite material has a room temperature yield strength of 794 MPa, a tensile strength of 1168 MPa, an elongation of 9%, and a microhardness of 357 HV.
[0071] Comparative Example 1
[0072] IN718 high-temperature alloy powder was placed in the grinding jar of a planetary ball mill, and anhydrous ethanol (99.5 wt.% purity) was added to completely submerge the powder. The particle size distribution of the IN718 high-temperature alloy powder was 15–53 μm. The grinding balls were made of 304 stainless steel, with a ball-to-powder mass ratio of 1:1, a rotation direction of 360°, a rotation speed of 200 r / min, and a grinding time of 6 h to ensure good sphericity. After ball milling, the resulting ball-milled system was subjected to ultrasonic vibration in an ultrasonic cleaner at a power of 65 W, for 30 min per cycle, twice with a 10 min interval. The ultrasonically treated product was then placed in a forced-air drying oven at 80℃ for 12 h, and sieved to obtain dried ball-milled powder with a particle size of 15–53 μm.
[0073] Based on the characteristics of laser powder bed fusion forming, a model was designed on a computer using 3D modeling software, saved as an STL file, and imported into the professional ARPS software of the laser powder bed fusion forming equipment for layering and slicing, and path planning. 304 stainless steel was selected as the substrate. During the laser powder bed fusion forming process, the substrate was preheated to 100℃, and 99.99wt.% high-purity argon gas was introduced as a protective gas, with an oxygen content below 300ppm.
[0074] The laser powder bed melting process parameters were set as follows: laser power of 250W, scanning rate of 833mm / s, layer thickness of 50μm, scanning spacing of 75μm, laser scanning mode of XY, and spot diameter of 75μm. The dried ball-milled powder prepared above was subjected to laser powder bed melting to obtain IN718 high-temperature alloy. Subsequently, the IN718 high-temperature alloy was cut from a 304 stainless steel substrate using wire electrical discharge machining.
[0075] Figure 6 This is a microstructure diagram of the IN718 high-temperature alloy prepared in Comparative Example 1 of this invention.
[0076] Using the same testing method as in Example 1, the room temperature yield strength of the IN718 high-temperature alloy prepared in Comparative Example 1 was 644 MPa, the tensile strength was 914 MPa, the elongation was 31%, and the microhardness was 330 HV.
[0077] Test case
[0078] By comparing the microstructures of the high-performance nickel-based superalloy / ceramic composite materials and IN718 superalloy prepared in Examples 1, 2 and Comparative Example 1, it can be seen that the addition of SiC significantly refines the grains of IN718 superalloy, playing a role in grain refinement and strengthening. The decomposition of SiC results in the presence of more silicides and MC carbides, which pin the grain boundaries and further improve the mechanical properties.
[0079] Figure 7 This is a comparison of the room temperature tensile curves of the high-performance nickel-based superalloy / ceramic composite materials and IN718 superalloy prepared in Examples 1, 2, and Comparative Example 1 of this invention. It can be seen that the IN718 / SiC prepared in Example 1... μm Composite material (IN718+2% SiC) μm Compared to the IN718 superalloy (IN718, laser power 250W) in Comparative Example 1, the yield strength of the IN718 / SiC alloy prepared in Example 2 (-250W) was increased by 20.19%, and the tensile strength was increased by 11.16%. nm Composite material (IN718+2% SiC) nm Compared to the IN718 high-temperature alloy (IN718-250W) in Comparative Example 1, the yield strength of IN718-250W is increased by 23.29% and the tensile strength is increased by 27.79%.
[0080] Figure 8 This image shows a comparison of the microhardness of the high-performance nickel-based superalloy / ceramic composite material and IN718 superalloy prepared by changing the laser power in Examples 1, 2, and Comparative Example 1. It can be seen that, based on Example 1, the IN718 / SiC prepared by adjusting the laser power to 200W and 300W... μm The microhardness of the composite material was increased by 8.18%, 7.58%, and 6.75% compared to the IN718 superalloy prepared under the corresponding laser power in Comparative Example 1, respectively. Based on Example 2, IN718 / SiC composites were prepared by adjusting the laser power to 200W and 300W. nm Compared with the IN718 high-temperature alloy prepared under the corresponding laser power in Comparative Example 1, the microhardness of the composite material was increased by 9.70%, 8.18%, and 16.56%, respectively.
[0081] The results of the examples show that the IN718 / SiC prepared in this invention... μmThe composite material exhibits a room temperature yield strength ≥750 MPa, tensile strength ≥1000 MPa, and hardness ≥345 HV. Compared to the deposited hardness of IN718 with 5% Al (CN116604031A), this represents a 5.03% increase. Compared to the yield strength of IN718 with CoAl2O4 added, as reported in the literature, the yield strength is increased by 8.71%, while the tensile strength remains comparable. Compared to the IN718 nickel-based superalloy, the yield strength is increased by 20.19%, the tensile strength by 11.16%, and the hardness by 7.58%. IN718 / SiC nm The composite material has a room temperature yield strength ≥770MPa, tensile strength ≥1030MPa, and hardness ≥355HV. Compared with IN718 with added CoAl2O4 in the literature, the yield strength is increased by 11.52% and the tensile strength is increased by 15.07%. Compared with IN718 nickel-based superalloy, the yield strength is increased by 23.29%, the tensile strength is increased by 27.79%, and the hardness is increased by 8.18%, as shown in Table 2.
[0082] Table 2 Comparison of the effects of the present invention and the prior art
[0083]
[0084] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing high-performance nickel-based superalloy / ceramic composite materials using laser powder bed melting technology, specifically comprising the following steps: Irregularly shaped SiC powder and IN718 high-temperature alloy powder were placed in the grinding jar of a planetary ball mill, and anhydrous ethanol with a purity of 99.5 wt.% was added to completely submerge the powder. The particle size distribution of the irregularly shaped SiC powder was 0.63~1.03 μm, and the particle size distribution of the IN718 high-temperature alloy powder was 15~53 μm. The mass of the irregularly shaped SiC powder was 2.0% of the total mass of the irregularly shaped SiC powder and IN718 high-temperature alloy powder. The added grinding balls... The material is 304 stainless steel. The ball-to-material mass ratio is controlled at 3:
1. The rotation direction is 360°, the rotation speed is 300 r / min, and the ball milling time is 4 h. After the ball milling is completed, the resulting ball milling system is subjected to ultrasonic vibration in an ultrasonic cleaner. The ultrasonic vibration power is 65W, each ultrasonic vibration lasts for 30 min, and the ultrasonic vibration is repeated 4 times with an interval of 10 min. The ultrasonically processed product is placed in a forced-air drying oven at a drying temperature of 80℃ for 12 h. After sieving, a dried mixed powder with a particle size of 15~55μm is obtained. Based on the characteristics of laser powder bed melting, a model was designed on a computer using 3D modeling software and saved in STL format. This model was then imported into the professional ARPS software for laser powder bed melting equipment for layering and slicing, and path planning was performed. 304 stainless steel was selected as the substrate. During the laser powder bed melting process, the substrate was preheated to 100°C, and 99.99 wt.% high-purity argon gas was introduced as a protective gas, with an oxygen content below 300 ppm. The laser powder bed melting process parameters were set as follows: laser power 250W, scanning rate 833 mm / s, layer thickness 50 μm, scanning spacing 75 μm, laser scanning mode XY, and spot diameter 75 μm. The dried mixed powder was then subjected to laser powder bed melting to obtain IN718 / SiC. nm Composite materials.
Citation Information
Patent Citations
TiB2 particle reinforced nickel-based cast superalloy and preparation method thereof
CN112522564A
Method for improving hardness of laser additive manufacturing In 718 alloy