Method for preparing humic acid-containing water-soluble silicon-potassium fertilizer by thermal catalysis of silicon-rich biomass solid waste
By using iron nanocatalysts under low-temperature catalytic pyrolysis conditions, silicon-rich biomass solid waste is converted into humic acid-containing water-soluble silicon-potassium fertilizer, which solves the problems of low effective silicon fertilizer content in biomass solid waste and complex humic acid production, achieving efficient conversion and resource recycling, and improving agricultural and economic benefits.
Patent Information
- Application Number
- CN202311854029.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-29
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-12-29
AI Technical Summary
In existing technologies, the effective silicon fertilizer content of biomass solid waste is low, the synthesis process is complex and costly, and the production of humic acid suffers from problems such as complex products, high energy consumption and low economic benefits. Furthermore, the silicon resources of biomass solid waste have not been effectively utilized.
Using iron nanocatalysts under low-temperature catalytic pyrolysis conditions, silicon-rich biomass solid waste is converted into humic acid-containing water-soluble silicon-potassium fertilizer. The organic matter conversion is promoted by atmospheric controlled oxygen catalytic roasting-oxidation method, and the catalyst is recovered by magnetic separation. Activators and extractants are added to improve the yield of humic acid and soluble silicon.
It achieves efficient conversion of organic matter in silicon-rich biomass solid waste, increases the yield of humic acid and soluble silicon, reduces costs, and provides nutrients such as N, P, and K, resulting in high agricultural and economic benefits and realizing a silicon cycle from soil to crops to soil.
Smart Images

Figure CN117986047B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of biomass solid waste resource utilization, and in particular to a method for the thermocatalytic production of humic acid-containing water-soluble silicon-potassium fertilizer from silicon-rich biomass solid waste. Background Technology
[0002] Globally, over 100 billion tons of agricultural biomass are generated annually. As one of the world's major agricultural countries, China generates a large amount of agricultural biomass solid waste each year, including rice husks, straw, nut shells, and stalks. However, currently, a large amount of biomass waste is mainly disposed of through incineration, which releases significant amounts of greenhouse gases. Therefore, innovative strategies and approaches are urgently needed to utilize biomass solid waste at high value.
[0003] Crops such as bamboo, rice, and reeds require large amounts of silicon during their growth, resulting in significant silicon content in the biomass solid waste generated from these crops. Silicon is a crucial nutrient element in plant matter, considered the fourth most abundant element after nitrogen, phosphorus, and potassium. It is an essential component of plant cell walls, enhancing crop resistance to lodging, pests, and diseases, increasing yield, improving quality, and enhancing the effectiveness of phosphate fertilizers. However, current compound silicon fertilizers contain relatively low levels of available silicon, and their synthesis involves complex processes and high costs. Therefore, the recycling of available silicon from silicon-rich biomass solid waste would be of paramount importance.
[0004] Humic acid is an important and relatively expensive organic fertilizer that has enjoyed high market recognition for many years. Traditionally, it is produced from weathered coal and lignite using an alkaline extraction method. However, high-humic-acid-content weathered coal and lignite resources are relatively scarce, resulting in limited production and persistently high market prices. Consequently, the technology of producing biochemical humic acid from biomass solid waste has begun to develop. However, composting for biochemical humic acid production suffers from unstable fertilizer efficiency and low economic returns; hydrothermal production presents stringent conditions and high costs; and rapid pyrolysis production results in complex products and high energy consumption. To address the current problems in the production of biochemical humic acid from biomass, CN202211344371.2 discloses a method for producing water-soluble fertilizer containing supermineral humic acid from agricultural and forestry biomass solid waste using low-temperature roasting; CN202211629558.7 discloses a method for converting traditional Chinese medicine residue into organic fertilizer using a cobalt-iron catalyst, employing pyrolysis activation with a cobalt-iron catalyst. Therefore, low-temperature catalytic pyrolysis can effectively convert biomass organic matter into humic acid, and it is cost-effective, making it promising for industrial-scale production.
[0005] Therefore, in view of the current problems with silicon fertilizer and based on the feasibility of low-temperature catalytic pyrolysis, a method is developed to realize the conversion of organic matter from silicon-rich biomass solid waste into humic acid while simultaneously utilizing the effective silicon. This method has high economic and environmental benefits. Summary of the Invention
[0006] The primary objective of this invention is to overcome the shortcomings and deficiencies of existing technologies by providing a method for the thermocatalytic production of humic acid-containing water-soluble silicon-potassium fertilizer from silicon-rich biomass solid waste.
[0007] Another objective of this invention is to provide the application of iron nanocatalysts in the preparation of humic acid-containing water-soluble silicon-potassium fertilizer.
[0008] The objective of this invention is achieved through the following technical solution:
[0009] An application of an iron nanocatalyst in the preparation of humic acid-containing water-soluble silicon-potassium fertilizer; the preparation method of the iron nanocatalyst includes the following steps: mixing iron salt and precipitant in water and hydrolyzing at 60-100℃ for 1-2 hours, then adding ferrous salt and pH adjuster to adjust the pH to neutral, and refluxing at boiling point for 1-2 hours to obtain the iron nanocatalyst.
[0010] Preferably, the molar ratio of the precipitant and the iron salt is 1:2.
[0011] Preferably, the molar ratio of the ferrous salt to the ferric salt is 1:4.
[0012] Preferably, the molar concentration of the iron salt in water is 0.4 mol / L.
[0013] Preferably, the iron salt includes at least one of ferric chloride, ferric nitrate, and ferric sulfate.
[0014] Preferably, the precipitant includes at least one of NH4OH and NaOH.
[0015] Preferably, the ferrous salt includes at least one of ferrous chloride, ferrous nitrate, and ferrous sulfate.
[0016] Preferably, the pH adjuster includes at least one of KOH and NaOH.
[0017] Preferably, all steps of the preparation method are carried out under N2 conditions.
[0018] A method for producing humic acid-containing water-soluble silicon-potassium fertilizer from silicon-rich biomass solid waste via thermocatalysis includes the following steps:
[0019] (1) The above iron nanocatalyst is mixed evenly with silicon-rich biomass solid waste and activator, and calcined at 200-400℃ in an atmosphere with a nitrogen to oxygen ratio of 9:1-3:1 for 3-5 hours to obtain weathered coal precursor.
[0020] (2) The weathered coal precursor obtained in step (1) is mixed with an aqueous solution of oxidant and oxidized at 60-100℃ for 8-12 hours. Then an extractant is added to separate the solid and liquid components. The resulting liquid is a water-soluble silicon-potassium fertilizer product containing humic acid.
[0021] Preferably, the silicon-rich biomass solid waste in step (1) includes at least one of bamboo, rice husks, reeds and plant straw; the plant straw includes at least one of rice, sugarcane and corn stalks.
[0022] Preferably, the silicon-rich biomass solid waste in step (1) is silicon-rich biomass solid waste powder, more preferably it is silicon-rich biomass solid waste powder obtained by washing and crushing silicon-rich biomass solid waste; most preferably, the silicon-rich biomass solid waste powder is silicon-rich biomass solid waste powder that has passed through a 200-mesh sieve.
[0023] Preferably, the amount of catalyst used in step (1) is 0.5% to 2% of the mass of silicon-rich biomass solid waste powder; more preferably, it is 1%.
[0024] Preferably, the activator in step (1) includes at least one of K3PO4, K2SO4, KNO3, KNO2 and K2SO3.
[0025] Preferably, the amount of activator used in step (1) is 10% to 50% of the mass of the silicon-rich biomass solid waste powder; more preferably, it is 30%.
[0026] Preferably, the oxidant in step (2) includes at least one of H2O2, HNO3 and CH3COOOH.
[0027] Preferably, the amount of oxidant used in step (2) is 1% to 5% of the mass of the silicon-rich biomass solid waste powder, more preferably 2%.
[0028] Preferably, the mass fraction of the oxidant aqueous solution in step (2) is 1% to 5%; more preferably, it is 1%.
[0029] Preferably, the extractant in step (2) includes at least one of KOH, K2CO3 and K4P2O7.
[0030] Preferably, the amount of extractant used in step (2) is 5% to 20% of the mass of the silicon-rich biomass solid waste powder; more preferably, it is 10%.
[0031] Preferably, the humic acid-containing water-soluble silicon-potassium fertilizer liquid product described in step (2) is used as a water-soluble fertilizer after being concentrated or diluted.
[0032] Preferably, the method further includes the following steps:
[0033] (3) The solid residue obtained in step (2) is separated by magnetic separation to obtain iron nanocatalyst.
[0034] The principle of the method described in this invention is as follows:
[0035] In this invention, silicon-rich biomass solid waste such as bamboo, rice husks, reeds, and plant stalks (including rice, sugarcane, and corn stalks) is cleaned and crushed, then mixed with an activator and catalyst in a certain proportion and subjected to controlled-atmosphere catalytic roasting and carbonization to obtain a weathered coal precursor. The silicon in the precursor is activated. The catalyst primarily lowers the activation energy for the decomposition and polymerization of lignin, cellulose, and hemicellulose, thereby achieving carbon chain recombination and forming humic acid and its precursor. The activator further enhances the catalyst's effect, promotes the formation of organic functional groups, converts insoluble silicon into soluble silicon, and provides certain nutrients such as N, P, and K. The obtained weathered coal precursor is then mixed with an oxidant in a certain proportion for oxidation. The oxidant further oxidizes the precursor, converting it into potassium humate and enriching its functional groups. An extractant is then added to extract the product. The extractant further participates in the reaction, extracting humic acid and soluble silicon, and further supplementing nutrients such as N, P, and K. The obtained product is subjected to solid-liquid separation. The resulting liquid is a water-soluble silicon-potassium fertilizer containing humic acid. The solid residue is separated by magnetic separation to recover the added catalyst for reuse.
[0036] The present invention has the following advantages and effects compared with the prior art:
[0037] (1) The present invention adopts an atmosphere-controlled oxygen catalytic roasting-oxidation method, which enables the organic matter conversion rate in silicon-rich biomass solid waste to reach 50-70%. The process is simple, the cost is low, and it can be used on a large scale in industrial applications.
[0038] (2) The catalyst used in this invention is a nano-sized iron catalyst, which has extremely high catalytic activity and is conducive to promoting the stability of the pH value of the reaction environment. Moreover, it can be reused by magnetic separation. The catalyst and oxidant promote the decomposition and polymerization of organic matter in silicon-rich biomass, further improving the yield of humic acid and improving agricultural and economic benefits. At the same time, the activator and extractant used can provide the product with nutrients such as N, P, and K, further improving the agricultural and economic benefits of humic acid-containing water-soluble silicon potassium fertilizer.
[0039] (3) This invention realizes the effective utilization of silicon, which transforms insoluble silicon in silicon-rich biomass solid waste into soluble silicon, which enters the solution to obtain liquid silicon fertilizer containing humic acid, thus realizing the silicon cycle of soil-crop-soil. Attached Figure Description
[0040] Figure 1 This is a flowchart of the present invention;
[0041] Figure 2 The image shows the XRD pattern of the dedicated iron nanocatalyst obtained in Example 1.
[0042] Figure 3 The graph shows the cyclic stability of the dedicated iron nanocatalyst obtained in Example 1.
[0043] Figure 4 The Fourier transform infrared absorption spectrum of humic acid in the humic acid-containing water-soluble silicon-potassium fertilizer obtained in Example 1 is shown.
[0044] Figure 5 This is a comparison chart of crop planting using humic acid-containing water-soluble silicon-potassium fertilizer and commercial silicon fertilizer and humic acid fertilizer in Example 4. Detailed Implementation
[0045] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this description. The present invention can also be applied through other different specific embodiments. Without departing from the spirit of the present invention, various details of this specification can be modified or changed based on different viewpoints and applications.
[0046] Before further describing specific embodiments of the present invention, it should be understood that the scope of protection of the present invention is not limited to the specific embodiments described below; the terminology used in the embodiments of the present invention is for describing specific embodiments and not for limiting the scope of protection of the present invention; and all technical and scientific terms used in the present invention have the same meaning as commonly understood by those skilled in the art.
[0047] The present invention will be further described in detail below with reference to the embodiments and accompanying drawings, but the implementation of the present invention is not limited thereto.
[0048] Unless otherwise specified in the embodiments of the present invention, the conditions shall be performed in accordance with conventional conditions or conditions recommended by the manufacturer; the raw materials and reagents used without specified manufacturers shall be conventional products that can be purchased commercially.
[0049] The process of this invention is as follows Figure 1 As shown.
[0050] Example 1
[0051] (1) Under N2 conditions, 0.4 mol of ferric salt (35.97 g Fe(NO3)3, 32.5 g FeCl3) was dissolved in 1 L of water to prepare a 0.4 mol / L ferric salt solution. Then, 8 g of precipitant (NaOH) was added, and the mixture was stirred and hydrolyzed at 60–100 °C for 1–2 h. Next, 0.1 mol of ferrous salt (6.34 g FeCl2, 12.09 g Fe(NO3)2) and pH adjuster (NaOH) were added to adjust the pH to neutral. The mixture was then refluxed at boiling point for 1–2 h to obtain a specific iron nanocatalyst. The XRD pattern of the iron nanocatalyst is shown below. Figure 2 As shown.
[0052] (2) Weigh 10kg of silicon-rich biomass solid waste (bamboo), wash and crush it and pass it through a 200-mesh sieve, and mix it evenly with the catalyst (100g of special iron nano-catalyst) and activator (1kgK3PO4, 1kgK2SO4 and 1kgKNO3) obtained in step (1), and calcine it at 300℃ in an atmosphere with a nitrogen to oxygen ratio of 7:1 for 4h to obtain weathered coal precursor;
[0053] (3) The weathered coal precursor obtained in step (2) was mixed with an oxidant (10L of 1% H2O2 solution and 10L of 1% CH3COOOH solution) and oxidized at 80℃ for 10h to obtain a preliminary product. Then, an extractant (0.5kg KOH, 0.25kg K2CO3 and 0.25kg K4P2O7) was added and the solid and liquid were separated.
[0054] (4) The catalyst mixture obtained in step (3) and the carbonization residue were magnetically separated to recover 98.2 g of catalyst. The recovered catalyst was then subjected to steps (2) to (5) for stability testing. The results are as follows: Figure 3 As shown.
[0055] (5) The liquid obtained in step (3) is a humic acid-containing water-soluble silicon-potassium fertilizer product. After concentration and granulation, 9.6 kg of humic acid-containing water-soluble silicon-potassium fertilizer solid product (silicon content reaches 13.5%) is obtained, which meets the Class I quality standard of HG / T 5933-2021 "Humic Acid Organic-Inorganic Compound Fertilizer" and the NY / T 3829-2021 "Silicon-Containing Water-Soluble Fertilizer" standard. The results are shown in Tables 1 and 2. The Fourier transform infrared absorption spectrum of humic acid in the humic acid-containing water-soluble silicon-potassium fertilizer product is shown in Table 2. Figure 4 As shown.
[0056] In this embodiment, 10 kg of silicon-rich biomass solid waste was treated. The catalyst dosage was 100 g, the activator dosage was 3 kg, the oxidant dosage was approximately 2 kg, and the extractant dosage was 1 kg. After the reaction, magnetic separation yielded 98.2 g of a special iron catalyst and 9.6 kg of humic acid-containing water-soluble silicon-potassium fertilizer solid product (silicon content was 13.5%). The yield was calculated as 96% based on the formula: yield = mass of humic acid-containing water-soluble silicon-potassium fertilizer solid product / mass of silicon-rich biomass powder.
[0057] Table 1. Test Results of Technical Indicators for HG / T 5933-2021 "Humic Acid Organic-Inorganic Compound Fertilizer"
[0058]
[0059] Table 2 Test Results of Technical Indicators for NY / T 3829-2021 "Silicon-Containing Water-Soluble Fertilizers"
[0060]
[0061] Comparative Example 1
[0062] (1) Under N2 conditions, 0.4 mol of iron salt (35.97 g Fe(NO3)3, 32.5 g FeCl3) was dissolved in 1 L of water to prepare a 0.4 mol / L iron salt solution. Then, 8 g of precipitant (NaOH) was added and mixed and stirred. After hydrolysis at 60-100℃ for 1-2 h, 0.1 mol of ferrous salt (6.34 g FeCl2, 12.09 g Fe(NO3)2) and pH adjuster (NaOH) were added to adjust the pH to neutral. The solution was refluxed at boiling point for 1-2 h to obtain a special iron nanocatalyst.
[0063] (2) Weigh 10kg of silicon-rich biomass solid waste (bamboo), wash and crush it and pass it through a 200-mesh sieve, and mix it evenly with the catalyst (50g of special iron nano-catalyst and 50g of commercial iron oxide catalyst) and activator (1kg of K3PO4, 1kg of K2SO4 and 1kg of KNO3) obtained in step (1), and calcine it at 300℃ in an atmosphere with a nitrogen to oxygen ratio of 7:1 for 4h to obtain weathered coal precursor;
[0064] (3) The weathered coal precursor obtained in step (2) was mixed with an oxidant (10L of 1% H2O2 solution and 10L of 1% CH3COOOH solution) and oxidized at 80℃ for 10h to obtain a preliminary product. Then, an extractant (0.5kg KOH, 0.25kg K2CO3 and 0.25kg K4P2O7) was added and the solid and liquid were separated.
[0065] (4) The catalyst obtained in step (3) was mixed with the carbonization residue and magnetically separated to recover 97.4g of catalyst.
[0066] (5) The liquid obtained in step (3) is a humic acid-containing water-soluble silicon-potassium fertilizer product. After concentration and granulation, 7.9 kg of humic acid-containing water-soluble silicon-potassium fertilizer solid product (silicon content is 3.6%) is obtained, which meets the Class I quality of HG / T 5933-2021 "Humic Acid Organic-Inorganic Compound Fertilizer" standard, but does not meet the NY / T 3829-2021 "Silicon-Containing Water-Soluble Fertilizer" standard.
[0067] This embodiment treats 10 kg of silicon-rich biomass solid waste. The catalyst dosage is 100 g, activator dosage is 3 kg, oxidant dosage is approximately 2 kg, and extractant dosage is 1 kg. After the reaction, magnetic separation yields 97.4 g of iron catalyst and 7.9 kg of humic acid-containing water-soluble silicon-potassium fertilizer solid product (silicon content 3.6%). The yield is calculated as: yield = mass of humic acid-containing water-soluble silicon-potassium fertilizer solid product / mass of silicon-rich biomass powder, yielding 84%. Compared with Example 1, this example replaces a certain amount of dedicated iron nanocatalyst with an equal amount of commercial iron oxide catalyst. Testing revealed a significant decrease in pH compared to Example 1 (results shown in Table 3), a slight decrease in the amount of iron catalyst obtained through magnetic separation, and a decrease in the yield of humic acid-containing water-soluble silicon-potassium fertilizer solid product, along with a decrease in silicon content. This indicates that the self-made iron nanocatalyst is more conducive to humic acid production and silicon utilization.
[0068] Table 3. pH results before and after the reaction in Example 1 and Comparative Example 1.
[0069]
[0070] Example 2
[0071] (1) Under N2 conditions, 0.4 mol of iron salt (35.97 g Fe(NO3)3, 32.5 g FeCl3) was dissolved in 1 L of water to prepare a 0.4 mol / L iron salt solution. Then, 8 g of precipitant (NaOH) was added and mixed and stirred. After hydrolysis at 60-100℃ for 1-2 h, 0.1 mol of ferrous salt (6.34 g FeCl2, 12.09 g Fe(NO3)2) and pH adjuster (NaOH) were added to adjust the pH to neutral. The solution was refluxed at boiling point for 1-2 h to obtain a special iron nanocatalyst.
[0072] (2) Weigh 10kg of silicon-rich biomass solid waste (rice straw), wash and crush it and pass it through a 200-mesh sieve, and mix it evenly with the catalyst (100g of special iron nano-catalyst) and activator (1kgK3PO4, 1kgK2SO4 and 1kgKNO3) obtained in step (1), and calcine it at 300℃ in an atmosphere with a nitrogen to oxygen ratio of 7:1 for 4h to obtain weathered coal precursor;
[0073] (3) The weathered coal precursor obtained in step (2) was mixed with an oxidant (10L of 1% H2O2 solution and 10L of 1% CH3COOOH solution) and oxidized at 80℃ for 10h to obtain a preliminary product. Then, an extractant (0.5kg KOH, 0.25kg K2CO3 and 0.25kg K4P2O7) was added and the solid and liquid were separated.
[0074] (4) The catalyst obtained in step (3) was mixed with the carbonization residue and magnetically separated to recover 98.1g of catalyst.
[0075] (5) The liquid obtained in step (3) is a humic acid-containing water-soluble silicon-potassium fertilizer product. After concentration and granulation, 9.2 kg of humic acid-containing water-soluble silicon-potassium fertilizer solid product (silicon content is 17.2%) is obtained, which meets the Class I quality of HG / T 5933-2021 "Humic Acid Organic-Inorganic Compound Fertilizer" standard and NY / T 3829-2021 "Silicon-Containing Water-Soluble Fertilizer" standard.
[0076] This embodiment processes 10 kg of silicon-rich biomass solid waste. The catalyst dosage is 100 g, activator dosage is 3 kg, oxidant dosage is approximately 2 kg, and extractant dosage is 1 kg. After the reaction, magnetic separation yields 98.1 g of a dedicated iron catalyst and 9.2 kg of humic acid-containing water-soluble silicon-potassium fertilizer solid product (silicon content 17.2%). The yield is calculated as: yield = mass of humic acid-containing water-soluble silicon-potassium fertilizer solid product / mass of silicon-rich biomass powder, resulting in a yield of 92%. Compared to Example 1, the raw material in this embodiment is rice straw, which has a higher silicon content than bamboo. The resulting humic acid-containing water-soluble silicon-potassium fertilizer solid product also has a higher silicon content, demonstrating effective utilization.
[0077] Example 3
[0078] (1) Under N2 conditions, 0.4 mol of iron salt (35.97 g Fe(NO3)3, 32.5 g FeCl3) was dissolved in 1 L of water to prepare a 0.4 mol / L iron salt solution. Then, 8 g of precipitant (NaOH) was added and mixed and stirred. After hydrolysis at 60-100℃ for 1-2 h, 0.1 mol of ferrous salt (6.34 g FeCl2, 12.09 g Fe(NO3)2) and pH adjuster (NaOH) were added to adjust the pH to neutral. The solution was refluxed at boiling point for 1-2 h to obtain a special iron nanocatalyst.
[0079] (2) Weigh 10kg of silicon-rich biomass solid waste (rice husk), wash and crush it and pass it through a 200-mesh sieve, and mix it evenly with the catalyst (100g of special iron nano-catalyst) and activator (1kgK3PO4, 1kgK2SO4 and 1kgKNO3) obtained in step (1), and calcine it at 300℃ in an atmosphere with a nitrogen to oxygen ratio of 7:1 for 4h to obtain weathered coal precursor;
[0080] (3) The weathered coal precursor obtained in step (2) was mixed with an oxidant (10L of 1% H2O2 solution and 10L of 1% CH3COOOH solution) and oxidized at 80℃ for 10h to obtain a preliminary product. Then, an extractant (0.5kg KOH, 0.25kg K2CO3 and 0.25kg K4P2O7) was added and the solid and liquid were separated.
[0081] (4) The catalyst obtained in step (3) was mixed with the carbonization residue and magnetically separated to recover 98.2g of catalyst.
[0082] (5) The liquid obtained in step (3) is a humic acid-containing water-soluble silicon-potassium fertilizer product. After concentration and granulation, 9.8 kg of humic acid-containing water-soluble silicon-potassium fertilizer solid product (silicon content is 21.3%) is obtained, which meets the Class I quality of HG / T 5933-2021 "Humic Acid Organic-Inorganic Compound Fertilizer" standard and NY / T 3829-2021 "Silicon-Containing Water-Soluble Fertilizer" standard.
[0083] This embodiment processes 10 kg of silicon-rich biomass solid waste. The catalyst dosage is 100 g, activator dosage is 3 kg, oxidant dosage is approximately 2 kg, and extractant dosage is 1 kg. After the reaction, magnetic separation yields 98.2 g of a dedicated iron catalyst and 9.8 kg of humic acid-containing water-soluble silicon-potassium fertilizer solid product (silicon content 21.3%). The yield is calculated as: yield = mass of humic acid-containing water-soluble silicon-potassium fertilizer solid product / mass of silicon-rich biomass powder, yielding a yield of 98%. Compared to Examples 1 and 2, the raw material in this embodiment is rice husk, which has a higher silicon content than bamboo and rice straw. The resulting humic acid-containing water-soluble silicon-potassium fertilizer solid product also has a higher silicon content. Multiple examples demonstrate that this technical route can effectively utilize silicon in silicon-rich biomass solid waste raw materials.
[0084] Comparative Example 2
[0085] (1) Under N2 conditions, 0.4 mol of iron salt (35.97 g Fe(NO3)3, 32.5 g FeCl3) was dissolved in 1 L of water to prepare a 0.4 mol / L iron salt solution. Then, 8 g of precipitant (NaOH) was added and mixed and stirred. After hydrolysis at 60-100℃ for 1-2 h, 0.1 mol of ferrous salt (6.34 g FeCl2, 12.09 g Fe(NO3)2) and pH adjuster (NaOH) were added to adjust the pH to neutral. The solution was refluxed at boiling point for 1-2 h to obtain a special iron nanocatalyst.
[0086] (2) Weigh 10kg of silicon-rich biomass solid waste (rice husk), wash and crush it and pass it through a 200-mesh sieve, and mix it evenly with the catalyst (100g of special iron nano-catalyst) and activator (1kgK3PO4, 1kgK2SO4 and 1kgKNO3) obtained in step (1), and calcine it at 300℃ in air atmosphere for 4h to obtain weathered coal precursor;
[0087] (3) The weathered coal precursor obtained in step (2) was mixed with an oxidant (10L of 1% H2O2 solution and 10L of 1% CH3COOOH solution) and oxidized at 80℃ for 10h to obtain a preliminary product. Then, an extractant (0.5kg KOH, 0.25kg K2CO3 and 0.25kg K4P2O7) was added and the solid and liquid were separated.
[0088] (4) The catalyst obtained in step (3) was mixed with the carbonization residue and magnetically separated to recover 98.2g of catalyst.
[0089] (5) The liquid obtained in step (3) is a humic acid-containing water-soluble silicon-potassium fertilizer product. After concentration and granulation, 7.4 kg of humic acid-containing water-soluble silicon-potassium fertilizer solid product (silicon content is 18.9%) is obtained, which meets the Class I quality of HG / T 5933-2021 "Humic Acid Organic-Inorganic Compound Fertilizer" standard and NY / T 3829-2021 "Silicon-Containing Water-Soluble Fertilizer" standard.
[0090] This embodiment processes 10 kg of silicon-rich biomass solid waste. The catalyst dosage is 100 g, activator dosage is 3 kg, oxidant dosage is approximately 2 kg, and extractant dosage is 1 kg. After the reaction, magnetic separation yields 97.8 g of a dedicated iron catalyst and 7.4 kg of humic acid-containing water-soluble silicon-potassium fertilizer solid product (silicon content 18.9%). The yield is calculated as: yield = mass of humic acid-containing water-soluble silicon-potassium fertilizer solid product / mass of silicon-rich biomass powder, resulting in a yield of 74%. Compared to Example 3, this embodiment uses an air atmosphere, leading to a significant reduction in product mass after step 2 due to substantial thermal decomposition, resulting in a decrease in both the final product yield and quality.
[0091] Example 4
[0092] (1) Select plump, pest-free, and uniformly sized corn seeds, disinfect them, and conduct a growth experiment. Accurately weigh 1 kg of soil into a flowerpot.
[0093] (2) Each group contains 100 seeds. The seeds are mixed with equal amounts of commercial silicon fertilizer, humic acid fertilizer, and water-soluble silicon-potassium fertilizer containing humic acid prepared in Example 1. The seeds are then planted evenly in flower pots. After the seeds germinate, they are watered in a measured amount. The potted plants are placed in a greenhouse with 16 hours of light and a temperature of (26±2)℃, 8 hours of darkness and a temperature of (24±2)℃, and a relative humidity of 70%.
[0094] (3) Adjust soil moisture with deionized water and replenish soil moisture regularly using a weighing method to maintain a constant soil moisture level. Repeat the experiment three times, harvesting corn seedlings in the fourth week after sowing for comparison. The results are as follows: Figure 5 As shown in Table 4.
[0095] In this embodiment, corn seedlings cultured for four weeks using the humic acid-containing water-soluble silicon-potassium fertilizer prepared in Example 1 had a plant height of 24.37 cm and a root length of 14.01 cm, demonstrating better fertilizer efficiency than single commercial silicon fertilizers and humic acid fertilizers. This indicates that the humic acid-containing water-soluble silicon-potassium fertilizer prepared by this process has a high content of soluble active silicon and also contains a certain amount of humic acid, providing better growth stimulation for silicon-requiring plants such as corn.
[0096] Table 4 Results of the Maize Crop Growth Experiment in Example 4
[0097]
[0098] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. The application of an iron nanocatalyst in the preparation of humic acid-containing water-soluble silicon-potassium fertilizer; characterized in that, The preparation method of the iron nanocatalyst includes the following steps: iron salt and precipitant are mixed in water and hydrolyzed at 60-100℃ for 1-2 hours, then ferrous salt and pH adjuster are added to adjust the pH to neutral, and the mixture is refluxed at boiling point for 1-2 hours to obtain the iron nanocatalyst. All steps of the preparation method described herein are carried out under N2 conditions; The molar ratio of the precipitant and the iron salt is 1:2; The molar ratio of the ferrous salt to the ferric salt is 1:4; The precipitant includes at least one of NH4OH and NaOH.
2. The application according to claim 1, characterized in that, The molar concentration of the iron salt in water is 0.4 mol / L.
3. The application according to claim 1, characterized in that, The iron salts mentioned include at least one of ferric chloride, ferric nitrate, and ferric sulfate; The ferrous salts mentioned include at least one of ferrous chloride, ferrous nitrate, and ferrous sulfate; The pH adjuster includes at least one of KOH and NaOH.
4. A method for the thermocatalytic production of humic acid-containing water-soluble silicon-potassium fertilizer from silicon-rich biomass solid waste, characterized in that... Includes the following steps: (1) The iron nanocatalyst described in any one of claims 1 to 3 is mixed evenly with silicon-rich biomass solid waste and activator, and calcined at 200 to 400°C in an atmosphere with a nitrogen to oxygen ratio of 9:1 to 3:1 for 3 to 5 hours to obtain a weathered coal precursor. (2) The weathered coal precursor obtained in step (1) is mixed with an aqueous solution of oxidant and oxidized at 60-100℃ for 8-12 hours. Then an extractant is added to separate the solid and liquid components. The resulting liquid is a water-soluble silicon potassium fertilizer product containing humic acid.
5. The method according to claim 4, characterized in that, The silicon-rich biomass solid waste mentioned in step (1) includes at least one of bamboo, rice husk, reed and plant straw; The silicon-rich biomass solid waste mentioned in step (1) is silicon-rich biomass solid waste powder; The activator in step (1) includes at least one of K3PO4, K2SO4, KNO3, KNO2 and K2SO3.
6. The method according to claim 4, characterized in that, The amount of catalyst used in step (1) is 0.5% to 2% of the mass of the silicon-rich biomass solid waste powder; The amount of activator used in step (1) is 10% to 50% of the mass of silicon-rich biomass solid waste powder.
7. The method according to claim 4, characterized in that, The oxidant in step (2) includes at least one of H2O2, HNO3, and CH3COOOH; The extractant in step (2) includes at least one of KOH, K2CO3 and K4P2O7.
8. The method according to claim 4, characterized in that, The amount of oxidant used in step (2) is 1% to 5% of the mass of the silicon-rich biomass solid waste powder; The mass fraction of the oxidant aqueous solution in step (2) is 1% to 5%; the amount of extractant used in step (2) is 5% to 20% of the mass of the silicon-rich biomass solid waste powder.
9. The method according to claim 4, characterized in that, The method further includes the following steps: (3) The solid residue obtained in step (2) is separated by magnetic separation to obtain iron nanocatalyst.
Citation Information
Patent Citations
Method for preparing super mineral source-containing humic acid water-soluble fertilizer by utilizing agriculture and forestry biomass solid waste
CN115611683A
A method for converting Chinese medicine residue into Chinese herbal medicine organic fertilizer using cobalt-iron catalyst
CN115894106B
Development and use of an iron-based catalyst for implementing an oxidation-reduction process for substances to be reduced
US20100075390A1
Electrochemical synthesis of humic acid and other partially oxidized carbonaceous materials
US4592814A