Reactive hyperbranched polysiloxane, toughened epoxy resin system and preparation method and application thereof

By introducing reactive hyperbranched polysiloxanes into epoxy resin to generate oxazolidinone structures, the problems of high viscosity and decreased glass transition temperature during toughening were solved, achieving a toughening effect with high toughness and low viscosity.

CN117986519BActive Publication Date: 2026-11-24CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211324872.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-27
Publication Date
2026-11-24
Estimated Expiration
2042-10-27

AI Technical Summary

Technical Problem

Existing epoxy resin toughening methods result in problems such as high viscosity, decreased glass transition temperature, and migration of toughening components, making it difficult to meet the requirements of high-end fields for excellent comprehensive performance.

Method used

The reactive hyperbranched polysiloxane, which contains rigid isocyanurate rings and flexible siloxane segments, reacts with epoxy resin during the curing process to form an oxazolidinone structure, which enhances intramolecular voids, improves toughness, maintains low viscosity, and prevents migration.

Benefits of technology

It significantly improves the toughness of epoxy resin systems, maintains low viscosity and glass transition temperature, avoids performance degradation, and is suitable for composite material processing and coating processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention provides a reactive hyperbranched polysiloxane, a toughened epoxy resin system, its preparation method, and its application. The reactive hyperbranched polysiloxane comprises a rigid isocyanurate ring and flexible siloxane segments, with terminal isocyanate groups. It is prepared from raw materials including hydroxyl polysiloxane, isocyanate trimer, diisocyanate, and a capping agent. The reactive hyperbranched polysiloxane prepared by this invention can significantly improve the toughness of the epoxy resin system without significantly increasing the system viscosity or drastically reducing the glass transition temperature of the cured epoxy resin system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of resins, and more specifically, to a reactive hyperbranched polysiloxane, toughened epoxy resin system, its preparation method, and its application. Background Technology

[0002] Advanced resin-based composites possess high specific modulus and specific strength, fatigue resistance, corrosion resistance, and strong design flexibility, leading to their widespread application in aerospace, military, automotive lightweighting, and many other fields, with their usage increasing daily. Resin plays a crucial role in load-bearing and load transfer in carbon fiber composites. Besides significantly influencing the mechanical properties of carbon fiber composites, resin also directly affects the composite's service temperature, resistance to damp heat, and weather resistance. Epoxy curing systems are among the most commonly used resin systems for resin-based composites. To improve the system's heat resistance, the selected epoxy resin and curing agent typically possess a high degree of rigidity and a high crosslinking density. To enhance the toughness of epoxy resin-based composites, the epoxy resin matrix is ​​usually toughened.

[0003] Different methods are used domestically and internationally to toughen and modify epoxy resins, such as using rubber elastomers, thermoplastic resins, and nanoparticles to toughen epoxy resin systems. These methods can effectively increase the toughness of epoxy resin systems, but often sacrifice other excellent properties, making it difficult to meet the new requirements for superior comprehensive performance in high-end applications. While rubber-toughened resin matrices can significantly improve the system's toughness, the low glass transition temperature and modulus of liquid rubber can also negatively impact the epoxy resin system. When the amount of rubber added is small, the improvement in system toughness is limited; increasing the amount of rubber, while significantly improving toughness, also leads to varying degrees of decrease in tensile strength, tensile modulus, and glass transition temperature. Introducing thermoplastic polymers into epoxy resin formulations can significantly improve the system's toughness without lowering the glass transition temperature. However, the dissolution of thermoplastic polymers in epoxy resins significantly increases the system's viscosity, altering the processing properties of the epoxy resin system. In nanomaterial-toughened epoxy resin systems, the dispersion of nanomaterials in epoxy resin is prone to agglomeration, which limits the amount of nanomaterials used in the epoxy system and leads to an increase in the viscosity of the epoxy resin system.

[0004] Hyperbranched polymers, due to their unique branched molecular structure, introduce intramolecular vacancies into the system, increasing the total free volume fraction. When the cured system is subjected to external forces, the chain segments near the vacancies can be disturbed, thereby consuming impact energy and improving the toughness of the system. In addition, the end groups can be designed to allow hyperbranched polymers to participate in the network of the epoxy curing system, solving the problems of decreased glass transition temperature and toughening agent migration caused by added toughening agents. Hyperbranched polymers also have the advantage of low viscosity, which can solve the problem of increased viscosity of epoxy systems caused by toughening agents.

[0005] Therefore, in order to address the shortcomings of traditional toughening methods for epoxy resin systems, a method for modifying epoxy resin systems with reactive hyperbranched polysiloxanes is needed. Summary of the Invention

[0006] To address the technical problems existing in the prior art, this invention provides a reactive hyperbranched polysiloxane and toughened epoxy resin system, its preparation method, and its application.

[0007] To address the problems of high viscosity, decreased glass transition temperature, and migration of toughening components in existing toughened epoxy resin systems, this invention provides a reactive hyperbranched polysiloxane comprising rigid isocyanurate rings and flexible siloxane segments. The reactive hyperbranched polysiloxane is inactive with epoxy resin at room temperature. During the curing process of the epoxy resin system, it reacts with the epoxy resin to generate an oxazolidinone structure. The intramolecular voids of the hyperbranched structure increase the free volume of the system. When the resin is subjected to impact, the reactive hyperbranched polysiloxane can absorb energy through segmental movement, significantly improving the toughness of the epoxy resin system without drastically increasing the viscosity or decreasing the glass transition temperature of the cured epoxy resin. The reactive hyperbranched polysiloxane does not migrate within the cured epoxy resin system, thus preventing performance degradation. Furthermore, it has low requirements for mixing and subsequent coating processes and provides good fiber impregnation effects.

[0008] One of the objectives of this invention is to provide a reactive hyperbranched polysiloxane.

[0009] The reactive hyperbranched polysiloxane comprises a rigid isocyanurate ring and a flexible siloxane segment, with the terminal end being an isocyanate group.

[0010] The reactive hyperbranched polysiloxane is not reactive with epoxy resin at room temperature, but reacts with epoxy resin during the curing process of the epoxy resin system to form an oxazolidinone structure.

[0011] In a preferred embodiment of the present invention, The reactive hyperbranched polysiloxane is prepared from raw materials including hydroxyl polysiloxane, isocyanate trimer, diisocyanate, and end-capping agent; In a preferred embodiment of the present invention, The hydroxyl polysiloxane has hydroxyl groups at both ends; preferably, the weight-average molecular weight of the hydroxyl polysiloxane is 200-5000, more preferably 200-1500. The isocyanate trimer is at least one of toluene diisocyanate trimer, isophorone diisocyanate trimer, diphenylmethane diisocyanate trimer, dicyclohexylmethane diisocyanate trimer, hexamethylene diisocyanate trimer, lysine diisocyanate trimer, and polymethylene polyphenyl polyisocyanate trimer. The diisocyanate is at least one selected from toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, and lysine diisocyanate. The capping agent is at least one of phenols, alcohols, lactams, dicarbonyl hydrogen, oximes, and sodium bisulfite capping agents, combined with an imidazole capping agent or at least one of imidazole capping agents; preferably, the capping agent is a combination of at least one of oxime capping agents and phenolic capping agents, combined with an imidazole capping agent. The imidazole-based end-capping agent is preferably at least one selected from imidazole, 2-methylimidazolium, 2-ethyl-4-methylimidazolium, 2-undecylimidazolium, 2-heptadecylimidazolium, 2-phenylimidazolium, and 2-phenyl-4-methylhydroxymethylimidazolium, more preferably at least one selected from imidazole, 2-methylimidazolium, and 2-ethyl-4-methylimidazolium; the oxime-based end-capping agent is preferably at least one selected from acetone oxime and butanone oxime; and the phenolic end-capping agent is preferably p-nitrophenol.

[0012] In a preferred embodiment of the present invention, The hydroxyl polysiloxane reacts with the isocyanate trimer to obtain a hydroxyl-terminated branched polysiloxane; the molar ratio of the hydroxyl groups of the hydroxyl polysiloxane to the isocyanate groups of the isocyanate trimer is (1.6~2.5):1, preferably (1.8~2.3):1.

[0013] In a preferred embodiment of the present invention, The diisocyanate reacts with the hydroxyl-terminated branched polysiloxane to obtain isocyanate-terminated branched polysiloxane; the molar ratio of the isocyanate group of the diisocyanate to the hydroxyl group of the hydroxyl-terminated branched polysiloxane is (1.5~2.4):1, preferably (1.7~2.2):1.

[0014] In a preferred embodiment of the present invention, The end-capping agent reacts with the isocyanate-terminated branched polysiloxane to obtain the reactive hyperbranched polysiloxane; the molar ratio of the end-capping agent to the isocyanate-terminated branched polysiloxane is (0.7~1.4):1, preferably (0.9~1.2):1.

[0015] A second objective of this invention is to provide a method for preparing reactive hyperbranched polysiloxanes, comprising the following steps: (1) Under the protection of a protective gas, the hydroxyl-terminated branched polysiloxane solution is reacted with the isocyanate trimer solution to obtain hydroxyl-terminated branched polysiloxane; (2) Under the protection of a protective gas, the hydroxyl-terminated branched polysiloxane obtained in step (1) is reacted with the diisocyanate solution to obtain isocyanate-terminated branched polysiloxane.

[0016] (3) Under the protection of a protective gas, the isocyanate-terminated branched polysiloxane obtained in step (2) is reacted with the terminator solution to obtain the reactive hyperbranched polysiloxane.

[0017] Step (3) requires the complete sealing of isocyanate groups in the system. Infrared or other monitoring methods can be used to confirm that all isocyanate groups have been reacted.

[0018] In a preferred embodiment of the present invention, Step (1), add catalyst A; the amount of catalyst A is preferably 0.5~3wt% of the mass of the isocyanate trimer, more preferably 1.5~2wt%; and / or, Step (2), add catalyst B; the amount of catalyst B is preferably 0.5~3wt% of the mass of the diisocyanate, more preferably 1~2wt%; and / or, Step (3): Add catalyst C; the amount of catalyst C is preferably 1 to 5% of the molar amount of the capping agent, preferably 2 to 3%.

[0019] In a preferred embodiment of the present invention, Step (1), The mass percentage concentration of the hydroxyl polysiloxane solution is 10-70%, preferably 30-50%; The isocyanate trimer solution has a mass percentage concentration of 10-70%, preferably 30-50%; The solvents of the hydroxyl polysiloxane solution and the isocyanate trimer solution are each independently selected from at least one of chloroform, dichloromethane, toluene, xylene, ethyl acetate, butyl acetate, acetone, methyl ethyl ketone, cyclohexanone, tetrahydrofuran, and N,N-dimethylformamide, preferably selected from at least one of chloroform and toluene; The mixing method involves adding the isocyanate trimer solution dropwise to the hydroxyl polysiloxane solution; Step (2), The mass percentage concentration of the diisocyanate solution is 10-70%, preferably 30-50%; The solvent for the diisocyanate is at least one selected from chloroform, dichloromethane, toluene, xylene, ethyl acetate, butyl acetate, acetone, methyl ethyl ketone, cyclohexanone, tetrahydrofuran, and N,N-dimethylformamide, preferably at least one selected from chloroform, toluene, and ethyl acetate. The mixing method involves adding a hydroxyl-terminated branched polysiloxane solution dropwise to a diisocyanate solution; Step (3), The mass percentage concentration of the capping agent solution is 10-70%, preferably 30-50%; The solvent of the capping agent solution is at least one selected from chloroform, toluene, acetone, methyl ethyl ketone, cyclohexanone, and tetrahydrofuran, preferably at least one selected from chloroform, toluene, and tetrahydrofuran; The mixing method involves adding the end-capping agent solution dropwise into isocyanate-terminated branched polysiloxane.

[0020] In a preferred embodiment of the present invention, The protective gas is at least one of nitrogen and an inert gas; and / or, Catalyst A and catalyst B are each independently selected from at least one of stannous octoate, dibutyltin dilaurate, triethylenediamine, lead octoate, zinc naphthenate, and tetraisobutyl titanate; and / or, The catalyst C is at least one of organotin, tertiary amine, cyclohexylamine ester, and carboxylic acid metal salt; preferably at least one of stannous octoate, dibutyltin dilaurate, and triethylamine.

[0021] In a preferred embodiment of the present invention, Step (1): The reaction temperature is 60~100℃, preferably 80~90℃, and the reaction time is 1~5h, preferably 2~3h; and / or, Step (2): The reaction temperature is 60~120℃, preferably 80~100℃, and the reaction time is 1~5h, preferably 2~3h; and / or, Step (3) involves a reaction temperature of 40-100℃, preferably 80-90℃, and a reaction time of 1-3h, preferably 2-3h.

[0022] A third objective of this invention is to provide a toughened epoxy resin system.

[0023] The toughened epoxy resin system includes the reactive hyperbranched polysiloxane, epoxy resin and its modified products, and curing agent.

[0024] In a preferred embodiment of the present invention, Based on 100 parts by weight of epoxy resin and its modified products, 100 parts by weight of epoxy resin and its modified products; 5-60 parts by weight of reactive hyperbranched polysiloxane; preferably 10-25 parts by weight; 10-40 parts by weight of curing agent; preferably 15-30 parts by weight.

[0025] In a preferred embodiment of the present invention, The epoxy resin and its modified products are at least one of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidylamine epoxy resin, alicyclic epoxide, and linear aliphatic epoxide; preferably at least one of bisphenol A epoxy resin, phenolic epoxy resin, bisphenol F epoxy, N,N-diglycidyl-4-glycidyloxyaniline, and 4,5-epoxyhexane-1,2-dicarboxylic acid diglycidyl ester. The curing agent is at least one of amine curing agents, acid anhydride curing agents, linear phenolic curing agents, polyester resin curing agents, polyurethane curing agents, styrene-maleic anhydride copolymer resin curing agents, and polysulfide rubber curing agents; preferably at least one of 4,4'-diaminodiphenyl sulfone, diaminodiphenylmethane, and dicyandiamide.

[0026] Optionally, the toughened epoxy resin system may also include other additives commonly used in the art, such as flame retardants, colorants, and water-resistant additives, in the usual amounts.

[0027] The fourth objective of this invention is to provide a method for preparing a toughened epoxy resin system, comprising: mixing the raw materials uniformly according to the specified amounts to obtain the toughened epoxy resin system; the mixing temperature is preferably 30~110℃; more preferably 50~100℃.

[0028] The toughened epoxy resin system can be cured according to general methods in the art to obtain a cured resin product. The preferred curing temperature is 120~180℃, and the preferred curing time is 2~3h.

[0029] The fifth objective of this invention is to provide an application of a reactive hyperbranched polysiloxane and toughened epoxy resin system in the field of resin-based composite materials. However, the application is not limited to this.

[0030] The beneficial effects of this invention are: (1) The reactive hyperbranched polysiloxane of the present invention contains a rigid isocyanurate ring and a flexible siloxane segment. The intramolecular voids of the hyperbranched structure increase the free volume of the system. When the resin is impacted, the reactive hyperbranched polysiloxane can absorb energy through the movement of the chain segments, which can significantly improve the toughness of the epoxy resin system.

[0031] (2) The reactive hyperbranched polysiloxane of the present invention toughens the epoxy resin system, which can avoid a significant increase in the viscosity of the system and change the original processing performance.

[0032] (3) The reactive hyperbranched polysiloxane of the present invention has no reactivity with epoxy resin at room temperature. During the curing process of epoxy resin system, it reacts with epoxy resin to generate oxazolidinone structure. The reactive hyperbranched polysiloxane will not significantly reduce the glass transition temperature of epoxy resin system cured product, nor will it cause toughening components to migrate in epoxy resin curing system, thereby degrading the performance of epoxy system cured product.

[0033] This invention primarily addresses the problems of high viscosity, decreased glass transition temperature, and migration of toughening components in toughened epoxy resin matrices. The reactive hyperbranched polysiloxane of this invention comprises rigid isocyanurate rings and flexible siloxane segments. The hyperbranched molecular structure significantly enhances the toughness of the epoxy resin system. The low viscosity of the hyperbranched structure does not significantly increase the viscosity of the epoxy resin system and does not alter its conventional processing properties. During the curing of the epoxy resin system, the reactive hyperbranched polysiloxane reacts with the epoxy resin, participating in the curing network of the epoxy resin, preventing migration of the hyperbranched polysiloxane within the system, and does not significantly reduce the glass transition temperature of the epoxy resin system. The reactive hyperbranched polysiloxane can be used for toughening various epoxy resin systems. Detailed Implementation

[0034] The present invention will now be described in detail with reference to specific embodiments. It should be noted that the following embodiments are only used to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the content of the present invention are still within the scope of protection of the present invention.

[0035] All raw materials used in the specific embodiments of this invention are conventional commercially available raw materials.

[0036] Test method: After the toughened epoxy resin system was cured, the epoxy resin cured product was obtained. The impact strength of the sample was tested according to GB / T 2571-1995 standard. The glass ring transition temperature of the epoxy resin cured product was tested according to ISO 6721-11 standard. The viscosity of the epoxy resin before curing was tested using a cone-plate viscometer.

[0037]

Example 1

[0038] A 50% (w / w) solution of isophorone diisocyanate was prepared in chloroform. The molar ratio of the isocyanate group in isophorone diisocyanate to the hydroxyl group in the hydroxyl-terminated branched polysiloxane was 2:1. Dibutyltin dilaurate was added to the isophorone diisocyanate solution at 1 wt% of the isophorone diisocyanate. The mixture was heated to 40°C and stirred under nitrogen protection. The hydroxyl-terminated branched polysiloxane solution was then added dropwise. After the addition was complete, the temperature was raised to 80°C and the reaction was carried out for 3 hours to obtain isocyanate-terminated branched polysiloxane.

[0039] Butanone oxime and 2-ethyl-4-methylimidazole were dissolved separately in chloroform to prepare a 50% (w / w) solution. The molar ratio of butanone oxime to 2-ethyl-4-methylimidazole was 1:1, and the molar ratio of butanone oxime to 2-ethyl-4-methylimidazole and the isocyanate groups in the isocyanate-terminated branched polysiloxane was 1.05:1. Stannous octoate was added to the isocyanate-terminated branched polysiloxane solution at 2% of the sum of the molar amounts of butanone oxime and 2-ethyl-4-methylimidazole. The mixture was heated to 40°C and stirred under nitrogen protection. The butanone oxime solution and the 2-ethyl-4-methylimidazole solution were added dropwise sequentially. After the addition was complete, the temperature was raised to 80°C, and the reaction was stopped after 2 hours. The product was then rotary evaporated under reduced pressure to obtain the reactive hyperbranched polysiloxane.

[0040] 2) Preparation of toughened epoxy resin system 59 parts by weight of 671 bisphenol A epoxy resin; 41 parts by weight of 128 bisphenol A epoxy resin; 18 parts by weight of reactive hyperbranched polysiloxane; 18 parts by weight of diaminodiphenyl sulfone; All components were mixed and heated to 70°C to disperse them evenly to obtain a toughened epoxy resin system. The toughened epoxy resin is cured to obtain a cured product. The curing process is 120℃ / 1h-180℃ / 1h.

[0041] 3) Performance evaluation of epoxy resin cured products The impact strength of the sample was tested according to GB / T 2571-1995 standard, the glass ring transition temperature of the epoxy resin cured product was tested according to ISO 6721-11 standard, and the viscosity of the epoxy resin before curing was tested using a cone-plate viscometer. The results are shown in Table 1.

[0042]

Example 2

[0043] The performance of the epoxy resin system and its cured product was evaluated according to the method in Example 1, and the results are shown in Table 1.

[0044]

Example 3

[0045] The performance of the epoxy resin system and its cured product was evaluated according to the method in Example 1, and the results are shown in Table 1.

[0046]

Example 4

[0047] The performance of the epoxy resin system and its cured product was evaluated according to the method in Example 1, and the results are shown in Table 1.

Example 5

[0048] The performance of the epoxy resin system and its cured product was evaluated according to the method in Example 1, and the results are shown in Table 1.

[0049]

Example 6

[0050] The performance of the epoxy resin system and its cured product was evaluated according to the method in Example 1, and the results are shown in Table 1.

[0051]

Example 7

[0052] The performance of the epoxy resin system and its cured product was evaluated according to the method in Example 1, and the results are shown in Table 1.

[0053]

Example 8

[0054] The performance of the epoxy resin system and its cured product was evaluated according to the method in Example 1, and the results are shown in Table 1.

[0055]

Example 9

[0056] 59 parts by weight of 671 bisphenol A epoxy resin; 41 parts by weight of 128 bisphenol A epoxy resin; 12 parts by weight of reactive hyperbranched polysiloxane; 18 parts by weight of diaminodiphenyl sulfone; The performance of the epoxy resin system and its cured product was evaluated according to the method in Example 1, and the results are shown in Table 1.

[0057]

Example 10

[0058] 59 parts by weight of 671 bisphenol A epoxy resin; 41 parts by weight of 128 bisphenol A epoxy resin; 24 parts by weight of reactive hyperbranched polysiloxane; 18 parts by weight of diaminodiphenyl sulfone; The performance of the epoxy resin system and its cured product was evaluated according to the method in Example 1, and the results are shown in Table 1.

[0059]

Example 11

[0060] 59 parts by weight of 671 bisphenol A epoxy resin; 41 parts by weight of 128 bisphenol A epoxy resin; 18 parts by weight of reactive hyperbranched polysiloxane; 18 parts by weight of diaminodiphenylmethane; The performance of the epoxy resin system and its cured product was evaluated according to the method in Example 1, and the results are shown in Table 1.

[0061]

Example 12

[0062] Isophorone diisocyanate was prepared into a 30% (w / w) ethyl acetate solution. The molar ratio of the isocyanate group in isophorone diisocyanate to the hydroxyl group in the hydroxyl-terminated branched polysiloxane was 1.7:1. Dibutyltin dilaurate was added to the isophorone diisocyanate solution at 2 wt% of the isophorone diisocyanate. The mixture was heated to 40°C and stirred under nitrogen protection. The hydroxyl-terminated branched polysiloxane solution was then added dropwise. After the addition was complete, the temperature was raised to 100°C and reacted for 2 hours to obtain isocyanate-terminated branched polysiloxane.

[0063] Butanone oxime and 2-ethyl-4-methylimidazole were dissolved separately in tetrahydrofuran to prepare a 30% (w / w) solution. The molar ratio of butanone oxime to 2-ethyl-4-methylimidazole was 1:1, and the molar ratio of butanone oxime to 2-ethyl-4-methylimidazole and the isocyanate groups in the isocyanate-terminated branched polysiloxane was 0.9:1. Stannous octoate was added to the isocyanate-terminated branched polysiloxane solution at 3% of the sum of the molar amounts of butanone oxime and 2-ethyl-4-methylimidazole. The mixture was heated to 40°C and stirred under nitrogen protection. The butanone oxime solution and the 2-ethyl-4-methylimidazole solution were added dropwise sequentially. After the addition was complete, the temperature was raised to 90°C, and the reaction was stopped after 3 hours. The product was then rotary evaporated under reduced pressure to obtain the reactive hyperbranched polysiloxane.

[0064] 2) Preparation of toughened epoxy resin system 59 parts by weight of 671 bisphenol A epoxy resin; 41 parts by weight of 128 bisphenol A epoxy resin; 10 parts by weight of reactive hyperbranched polysiloxane; 15 parts by weight of diaminodiphenyl sulfone; All components were mixed and heated to 50°C to disperse them evenly, thus obtaining a toughened epoxy resin system. The toughened epoxy resin is cured to obtain a cured product. The curing process is 120℃ / 1h-180℃ / 1h.

[0065] 3) Performance evaluation of epoxy resin cured products The performance of the epoxy resin system and its cured product was evaluated according to the method in Example 1, and the results are shown in Table 1.

[0066]

Example 13

[0067] Isophorone diisocyanate was prepared into a 30% (w / w) ethyl acetate solution. The molar ratio of the isocyanate group in isophorone diisocyanate to the hydroxyl group in the hydroxyl-terminated branched polysiloxane was 2.2:1. Dibutyltin dilaurate was added to the isophorone diisocyanate solution at an amount of 2 wt% of the isophorone diisocyanate. The mixture was heated to 40°C and stirred under nitrogen protection. The hydroxyl-terminated branched polysiloxane solution was then added dropwise. After the addition was complete, the temperature was raised to 100°C and the reaction was carried out for 2 hours to obtain isocyanate-terminated branched polysiloxane.

[0068] Butanone oxime and 2-ethyl-4-methylimidazole were dissolved separately in tetrahydrofuran to prepare a 30% (w / w) solution. The molar ratio of butanone oxime to 2-ethyl-4-methylimidazole was 1:1, and the molar ratio of butanone oxime to 2-ethyl-4-methylimidazole and the isocyanate groups in the isocyanate-terminated branched polysiloxane was 1.2:1. Stannous octoate was added to the isocyanate-terminated branched polysiloxane solution at 3% of the sum of the molar amounts of butanone oxime and 2-ethyl-4-methylimidazole. The mixture was heated to 40°C and stirred under nitrogen protection. The butanone oxime solution and the 2-ethyl-4-methylimidazole solution were added dropwise sequentially. After the addition was complete, the temperature was raised to 90°C, and the reaction was stopped after 3 hours. The product was then rotary evaporated under reduced pressure to obtain the reactive hyperbranched polysiloxane.

[0069] 2) Preparation of toughened epoxy resin system 59 parts by weight of 671 bisphenol A epoxy resin; 41 parts by weight of 128 bisphenol A epoxy resin; 25 parts by weight of reactive hyperbranched polysiloxane; 30 parts by weight of diaminodiphenyl sulfone; All components were mixed and heated to 100°C to disperse them evenly to obtain a toughened epoxy resin system. The toughened epoxy resin is cured to obtain a cured product. The curing process is 120℃ / 1h-180℃ / 1h.

[0070] 3) Performance evaluation of epoxy resin cured products The performance of the epoxy resin system and its cured product was evaluated according to the method in Example 1, and the results are shown in Table 1.

[0071]

Comparative Example 1

[0072] The performance of the epoxy resin system and its cured product was evaluated according to the method in Example 1, and the results are shown in Table 1.

[0073] [Comparative Example 2] The epoxy resin cured product was prepared according to the method of Example 1, the difference from Example 1 being that: the reactive hyperbranched polysiloxane was prepared, and the isocyanate-terminated branched polysiloxane was not end-capped with an end-capping agent. Everything else is the same as in Example 1.

[0074] The performance of the epoxy resin system and its cured product was evaluated according to the method in Example 1, and the results are shown in Table 1.

[0075] [Comparative Example 3] The epoxy resin cured product was prepared according to the method of Example 1, the difference being that the raw materials required for the preparation of the viscosity-reducing reactive hyperbranched polysiloxane were directly mixed without reaction. Everything else is the same as in Example 1.

[0076] The performance of the epoxy resin system and its cured product was evaluated according to the method in Example 1, and the results are shown in Table 1.

[0077] [Comparative Example 4] The epoxy resin cured product was prepared according to the method of Example 1, the difference being that in Example 1, an equal amount of nitrile rubber was used to replace the reactive hyperbranched polysiloxane for toughening in the toughened epoxy resin system. Everything else is the same as in Example 1.

[0078] The performance of the epoxy resin system and its cured product was evaluated according to the method in Example 1, and the results are shown in Table 1.

[0079] [Comparative Example 5] The epoxy resin cured product was prepared according to the method of Example 1, the difference from Example 1 being that the reactive hyperbranched polysiloxane was replaced with an equal amount of thermoplastic polyethersulfone resin in the toughened epoxy resin system for toughening. Everything else is the same as in Example 1.

[0080] The performance of the epoxy resin system and its cured product was evaluated according to the method in Example 1, and the results are shown in Table 1.

[0081] Table 1. Test results of epoxy resin system and its cured product

[0082] Compared with Example 1, Comparative Example 1 does not contain reactive hyperbranched polysiloxanes; Comparative Example 2: Isocyanate-terminated branched polysiloxanes were not end-capped using an end-capping agent; In Comparative Example 3, the raw materials required for the preparation of reactive hyperbranched polysiloxanes were directly mixed without any reaction. Comparative Examples 4 and 5 replaced the reactive hyperbranched polysiloxane in Example 1 with equal amounts of nitrile rubber and thermoplastic polyethersulfone, respectively. The impact strength of Example 1 is 92 kJ / m 2 The glass transition temperature is 174℃, and the viscosity at 70℃ is 30 Pa·s; the impact strength of Comparative Examples 1 to 5 is 55 to 83 kJ / m. 2 Comparative Examples 3-4 had glass transition temperatures of 143-157°C, while Comparative Examples 2-3 and 5 had viscosities of 120-183 Pa·s at 70°C.

[0083] The impact strength of Examples 1-13 is 79-97 kJ / m. 2 The glass transition temperature is 163~179℃, and the viscosity at 70℃ is 29~36 Pa·s. The epoxy resins prepared in Examples 1~13 have high toughness and low viscosity, and will not significantly reduce the glass transition temperature of the epoxy resin system cured product, thus preventing the performance degradation of the epoxy system cured product. The reactive hyperbranched polysiloxane prepared in this invention can be used for toughening various epoxy resin systems.

Claims

1. A reactive hyperbranched polysiloxane, the reactive hyperbranched polysiloxane comprising a rigid isocyanurate ring and a flexible siloxane segment, the ends of which are capped isocyanate groups; the reactive hyperbranched polysiloxane is prepared by a method comprising the following steps: (1) Under the protection of a protective gas, a hydroxyl-terminated branched polysiloxane solution was reacted with an isocyanate trimer solution to obtain a hydroxyl-terminated branched polysiloxane. (2) Under the protection of a protective gas, the hydroxyl-terminated branched polysiloxane obtained in step (1) is reacted with a diisocyanate solution to obtain isocyanate-terminated branched polysiloxane. (3) Under the protection of a protective gas, the isocyanate-terminated branched polysiloxane obtained in step (2) is reacted with the end-capping agent solution to obtain the reactive hyperbranched polysiloxane.

2. The reactive hyperbranched polysiloxane as described in claim 1, characterized in that: The hydroxyl polysiloxane has hydroxyl groups at both ends; and / or, The isocyanate trimer is at least one selected from toluene diisocyanate trimer, isophorone diisocyanate trimer, diphenylmethane diisocyanate trimer, dicyclohexylmethane diisocyanate trimer, hexamethylene diisocyanate trimer, lysine diisocyanate trimer, and polymethylene polyphenyl polyisocyanate trimer; and / or, The diisocyanate is at least one selected from toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, and lysine diisocyanate; and / or, The capping agent is a combination of at least one of phenols, alcohols, lactams, dicarbonyl hydrogen, oximes, sodium bisulfite capping agents, and at least one of imidazole capping agents.

3. The reactive hyperbranched polysiloxane as described in claim 2, characterized in that: The weight-average molecular weight of the hydroxyl polysiloxane is 200-5000; and / or, The imidazole end-capping agent is at least one selected from imidazole, 2-methylimidazolium, 2-ethyl-4-methylimidazolium, 2-undecylimidazolium, 2-heptadecylimidazolium, 2-phenylimidazolium, and 2-phenyl-4-methylhydroxymethylimidazolium; the oxime end-capping agent is at least one selected from acetone oxime and butanone oxime; and the phenolic end-capping agent is p-nitrophenol.

4. The reactive hyperbranched polysiloxane as described in claim 3, characterized in that: The weight-average molecular weight of the hydroxyl polysiloxane is 200-1500.

5. The reactive hyperbranched polysiloxane as described in claim 1, characterized in that: The hydroxyl polysiloxane reacts with the isocyanate trimer to obtain a hydroxyl-terminated branched polysiloxane; the molar ratio of the hydroxyl groups of the hydroxyl polysiloxane to the isocyanate groups of the isocyanate trimer is (1.6~2.5):

1.

6. The reactive hyperbranched polysiloxane as described in claim 5, characterized in that: The molar ratio of the hydroxyl groups in the hydroxyl polysiloxane to the isocyanate groups in the isocyanate trimer is (1.8~2.3):

1.

7. The reactive hyperbranched polysiloxane as described in claim 5, characterized in that: The diisocyanate reacts with the hydroxyl-terminated branched polysiloxane to obtain isocyanate-terminated branched polysiloxane; the molar ratio of the isocyanate group of the diisocyanate to the hydroxyl group of the hydroxyl-terminated branched polysiloxane is (1.5~2.4):

1.

8. The reactive hyperbranched polysiloxane as described in claim 5, characterized in that: The molar ratio of the isocyanate group of the diisocyanate to the hydroxyl group of the hydroxyl-terminated branched polysiloxane is (1.7~2.2):

1.

9. The reactive hyperbranched polysiloxane as described in claim 7, characterized in that: The end-capping agent reacts with the isocyanate-terminated branched polysiloxane to obtain the reactive hyperbranched polysiloxane; the molar ratio of isocyanate groups in the end-capping agent and the isocyanate-terminated branched polysiloxane is (0.7~1.4):

1.

10. The reactive hyperbranched polysiloxane as described in claim 9, characterized in that: The molar ratio of the end-capping agent to the isocyanate-terminated branched polysiloxane is (0.9~1.2):

1.

11. A method for preparing a reactive hyperbranched polysiloxane according to any one of claims 1 to 10, the method comprising the following steps: (1) Under the protection of a protective gas, the hydroxyl-terminated branched polysiloxane solution is reacted with the isocyanate trimer solution to obtain hydroxyl-terminated branched polysiloxane; (2) Under the protection of a protective gas, the hydroxyl-terminated branched polysiloxane obtained in step (1) is reacted with the diisocyanate solution to obtain isocyanate-terminated branched polysiloxane. (3) Under the protection of a protective gas, the isocyanate-terminated branched polysiloxane obtained in step (2) is reacted with the terminator solution to obtain the reactive hyperbranched polysiloxane.

12. The method for preparing reactive hyperbranched polysiloxane as described in claim 11, characterized in that: Step (1), add catalyst A; and / or, Step (2), add catalyst B; and / or, Step (3), add catalyst C.

13. The method for preparing reactive hyperbranched polysiloxane as described in claim 12, characterized in that: In step (1), the amount of catalyst A is 0.5~3 wt% of the mass of the isocyanate trimer; and / or, In step (2), the amount of catalyst B is 0.5~3 wt% of the mass of the diisocyanate; and / or, In step (3), the amount of catalyst C used is 1 to 5% of the molar amount of the capping agent.

14. The method for preparing reactive hyperbranched polysiloxane as described in claim 13, characterized in that: In step (1), the amount of catalyst A is 1.5~2 wt% of the mass of the isocyanate trimer; and / or, In step (2), the amount of catalyst B is 1-2 wt% of the mass of the diisocyanate; and / or, In step (3), the amount of catalyst C used is 2 to 3% of the molar amount of the capping agent.

15. The method for preparing reactive hyperbranched polysiloxane as described in claim 11, characterized in that: Step (1), The mass concentration of the hydroxyl polysiloxane solution is 10-70%; and / or, The isocyanate trimer solution has a mass concentration of 10-70%; and / or, The solvents for the hydroxyl polysiloxane solution and the isocyanate trimer solution are independently selected from chloroform, dichloromethane, toluene, xylene, ethyl acetate, butyl acetate, acetone, methyl ethyl ketone, cyclohexanone, tetrahydrofuran, N,N-dimethylformamide; and / or, The isocyanate trimer solution is added dropwise to the hydroxyl polysiloxane solution; and / or Step (2), The mass concentration of the diisocyanate solution is 10-70%; and / or, The solvent for the diisocyanate is at least one selected from chloroform, dichloromethane, toluene, xylene, ethyl acetate, butyl acetate, acetone, methyl ethyl ketone, cyclohexanone, tetrahydrofuran, and N,N-dimethylformamide; and / or, The hydroxyl-terminated branched polysiloxane solution is added dropwise to the diisocyanate solution; and / or, Step (3), The mass concentration of the capping agent solution is 10-70%; and / or, The solvent of the capping agent solution is at least one selected from chloroform, toluene, acetone, methyl ethyl ketone, cyclohexanone, and tetrahydrofuran; and / or, The capping agent solution is added dropwise to isocyanate-capped branched polysiloxane.

16. The method for preparing reactive hyperbranched polysiloxane as described in claim 15, characterized in that: Step (1), The mass concentration of the hydroxyl polysiloxane solution is 30-50%; and / or, The isocyanate trimer solution has a mass concentration of 30-50%; and / or Step (2), The mass concentration of the diisocyanate solution is 30-50%; and / or, Step (3), The mass concentration of the capping agent solution is 30-50%.

17. The method for preparing reactive hyperbranched polysiloxane as described in claim 12, characterized in that: The protective gas is at least one of nitrogen and an inert gas; and / or, Catalyst A and catalyst B are each independently selected from at least one of stannous octoate, dibutyltin dilaurate, triethylenediamine, lead octoate, zinc naphthenate, and tetraisobutyl titanate; and / or, The catalyst C is at least one of organotin, tertiary amine, cyclohexylamine ester, and metal carboxylic acid salt.

18. The method for preparing reactive hyperbranched polysiloxane as described in claim 17, characterized in that: The catalyst C is at least one of stannous octoate, stannous dibutyldilaurate, and triethylamine.

19. The method for preparing reactive hyperbranched polysiloxane as described in claim 11, characterized in that: Step (1): The reaction temperature is 60~100℃, and the reaction time is 1~5h; and / or, Step (2), the reaction temperature is 60~120℃, and the reaction time is 1~5h; and / or, Step (3): The reaction temperature is 40~100℃ and the reaction time is 1~3h.

20. The method for preparing reactive hyperbranched polysiloxane as described in claim 19, characterized in that: Step (1): The reaction temperature is 80~90℃, and the reaction time is 2~3h; and / or, Step (2), the reaction temperature is 80~100℃, and the reaction time is 2~3h; and / or, Step (3): The reaction temperature is 80~90℃ and the reaction time is 2~3h.

21. A toughened epoxy resin system comprising the reactive hyperbranched polysiloxane according to any one of claims 1 to 10 or the reactive hyperbranched polysiloxane prepared by the method according to any one of claims 11 to 20, wherein the toughened epoxy resin system further comprises epoxy resin and its modified products, and curing agent.

22. The toughened epoxy resin system as described in claim 21, characterized in that: Based on 100 parts by weight of epoxy resin and its modified products, 100 parts by weight of epoxy resin and its modified products; 5-60 parts by weight of reactive hyperbranched polysiloxane; 10-40 parts by weight of curing agent.

23. The toughened epoxy resin system as described in claim 22, characterized in that: Based on 100 parts by weight of epoxy resin and its modified products, 100 parts by weight of epoxy resin and its modified products; 10-25 parts by weight of reactive hyperbranched polysiloxane; 15-30 parts by weight of curing agent.

24. The toughened epoxy resin system as described in claim 21, characterized in that: The epoxy resin and its modified products are at least one of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, alicyclic epoxide, and linear aliphatic epoxide; and / or, The curing agent is at least one of amine curing agents, acid anhydride curing agents, linear phenolic curing agents, polyester resin curing agents, polyurethane curing agents, and polysulfide rubber curing agents.

25. The toughened epoxy resin system as described in claim 24, characterized in that: The epoxy resin and its modified products are at least one selected from bisphenol A epoxy resin, phenolic epoxy resin, bisphenol F epoxy resin, N,N-diglycidyl-4-glycidyloxyaniline, and 4,5-epoxyhexane-1,2-dicarboxylic acid diglycidyl ester; and / or The curing agent is at least one of styrene-maleic anhydride copolymer resin curing agent, 4,4'-diaminodiphenyl sulfone, diaminodiphenylmethane, and dicyandiamide.

26. A method for preparing a toughened epoxy resin system as described in any one of claims 21 to 25, comprising: The toughened epoxy resin system is prepared by uniformly mixing the raw materials according to the specified amounts.

27. The method for preparing the toughened epoxy resin system as described in claim 26, characterized in that: The mixing temperature is 30~110℃.

28. The method for preparing the toughened epoxy resin system as described in claim 27, characterized in that: The mixing temperature is 50~100℃.

29. The application of a reactive hyperbranched polysiloxane as described in any one of claims 1 to 10 or a toughened epoxy resin system as described in any one of claims 21 to 25 in the field of resin-based composite materials.

Citation Information

Patent Citations

  • Terminal-carboxyl-group polyester resin modified epoxide resin, preparation method thereof, and electrophoretic paint and preparation method thereof

    CN108586756A