A method for preparing a cross-linked PI-PUU multi-fluorine block copolymer by a solvent-free method

The preparation of cross-linked PI-PUU polyfluorinated block copolymers by a solvent-free method solves the problems of water resistance and mechanical strength of polyurethane elastomers, and realizes a copolymer with high strength, toughness and wear resistance, which is suitable for processing a variety of materials.

CN117986596BActive Publication Date: 2026-11-24LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410076954.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-19
Publication Date
2026-11-24
Estimated Expiration
2044-01-19

AI Technical Summary

Technical Problem

Existing polyurethane elastomers suffer from poor water resistance, low mechanical strength, and poor wear resistance during service. Furthermore, the traditional synthesis process requires a large amount of organic solvents, which does not meet the requirements for green and environmentally friendly production.

Method used

Crosslinked PI-PUU polyfluorinated block copolymers were prepared using a solvent-free method. Diisocyanate, diol, difunctional aminobiphenyl and trifunctional aminophenylamine were mixed through a solvent-free polymerization reaction to form hyperbranched amino-terminated PUU molecular chains and linear isocyanate-terminated PI molecular chains, which were then crosslinked to form polyfluorinated block copolymers.

Benefits of technology

The prepared cross-linked PI-PUU polyfluorinated block copolymer has excellent water resistance and low coefficient of friction, as well as high mechanical strength and toughness, making it suitable for various material processing and molding processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117986596B_ABST
    Figure CN117986596B_ABST
Patent Text Reader

Abstract

This invention provides a solvent-free method for preparing cross-linked PI-PUU polyfluorinated block copolymers, relating to the field of polymer preparation technology. This invention prepares cross-linked PI-PUU polyfluorinated block copolymers via solution polymerization. The solvent-free method facilitates various material processing and molding techniques. Starting from relatively simple and readily available raw materials, this invention eliminates the need for intermediate separation and stringent imidization processes, directly obtaining polyimide-polyurethane copolymers. Because both the soft and hard segments of the copolymer contain a certain amount of fluorine atoms, the cross-linked PI-PUU polyfluorinated block copolymer exhibits excellent water resistance and a low coefficient of friction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer preparation technology, and specifically to a solvent-free method for preparing cross-linked PI-PUU polyfluorinated block copolymers. Background Technology

[0002] Polyurethane elastomers, due to their customizable mechanical strength, satisfactory toughness, and good elasticity, have attracted considerable attention and shown great promise in various fields such as actuators, soft robots, and flexible electronics. In particular, emerging sectors like the automotive industry and sporting goods have a significant demand for high-mechanical-strength elastomers. Polyurethane (PU) is a block polymer containing urethane (-NHCOO-) and composed of alternating soft and hard segments. The presence of numerous hydrogen bonds between the polymer chains inevitably leads to problems such as poor water resistance, low mechanical strength, and poor abrasion resistance during service, which affects the material's usability. For the development of a sustainable economy, researching polyurethane elastomers with high mechanical strength, combined with toughness and environmental adaptability is essential. However, manufacturing high-performance elastomers that simultaneously combine high mechanical strength, toughness, satisfactory tensile / elasticity, and excellent water resistance remains a significant challenge.

[0003] Triblock poly(styrene-butadiene-styrene) (SBS) is a widely used elastomer. Due to its unique two-phase structure, SBS exhibits excellent mechanical strength, tensile strength, and elasticity. In SBS elastomers, the polystyrene segments tend to separate from the elastic polybutadiene matrix to form a dispersed phase, thereby contributing to improved SBS strength. Simultaneously, the polybutadiene segments, as the continuous phase, possess soft properties, which further enhance the tensile strength and elasticity of SBS. Therefore, copolymers used to construct elastomers should consist of rigid segments that can assemble into highly rigid nanostructures, while soft segments should contain non-covalent crosslinking groups. Based on the design principles of SBS and previously reported mechanically robust and tough elastomers, Sun et al. (Z.Guo, X.Lu, X.Wang, X.Li, J.Li, J.Sun, Engineering of Chain Rigidity and Hydrogen Bond Cross-Linking toward Ultra-Strong, Healable, Recyclable, and Water-Resistant Elastomers. Adv. Mater. 2023, n / a(n / a), 2300286.) proposed that by strengthening the rigid phase-separated nanostructure and appropriately cross-linking the elastic matrix through reversible supramolecular interactions, reversibly cross-linked elastomers with ultra-high strength and toughness, and satisfactory tensile and elastic properties can be prepared. Compared with polystyrene in SBS, polyimide (PI) is more conducive to forming a more rigid phase-separated nanostructure, making it an ideal rigid segment for manufacturing mechanically robust and tough elastomers. Meanwhile, the hydrophobicity of PI chains is expected to endow the elastomer with excellent water resistance. On the other hand, poly(urea-urethane) (PUU) is generated by the addition reaction of polyisocyanates and multinucleophiles, containing both urea and amino groups. When used as a soft segment, the multiple hydrogen bonds on the PUU chain can be reversibly broken under external force, effectively dissipating energy and improving the strength and toughness of the elastomer. However, the commonly used PI synthesis process (dianhydride + diamine) usually requires the synthesis of polyimide acid first, followed by high-temperature (>180℃) imidization to obtain polyimide, which involves harsh synthesis conditions. Secondly, the synthesis process requires a large amount of organic solvents, which does not meet the current green and environmentally friendly production requirements of industrial production, and the presence of a large amount of solvent in the product is detrimental to material molding processes such as casting. Summary of the Invention

[0004] The purpose of this invention is to provide a solvent-free method for preparing cross-linked PI-PUU polyfluorinated block copolymers. This method eliminates the need for solvents and imidization, and introduces a large amount of fluorinated monomers into both the PUU and PI segments, increasing the fluorine content of the polymer. The cross-linked PI-PUU polyfluorinated block copolymer prepared by this invention possesses excellent strength, toughness, water resistance, and friction-reducing and wear-resistant properties.

[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution:

[0006] This invention provides a solvent-free method for preparing cross-linked PI-PUU polyfluorinated block copolymers, comprising the following steps:

[0007] Diisocyanate, diol and first catalyst are mixed and subjected to first polymerization reaction to obtain polyurethane prepolymer;

[0008] The polyurethane prepolymer, bifunctional aminobiphenyl and trifunctional aminophenylamine are mixed and subjected to a second polymerization reaction to obtain hyperbranched amino-terminated PUU molecular chains.

[0009] 4,4'-diisocyanate-3,3'-dimethylbiphenyl, acid anhydride, and a second catalyst were mixed and subjected to a third polymerization reaction to obtain linear isocyanate-terminated PI molecular chains.

[0010] The hyperbranched amino-terminated PUU molecular chains and the linear isocyanate-terminated PI molecular chains are mixed and subjected to a fourth polymerization reaction to obtain a cross-linked PI-PUU polyfluorinated block copolymer.

[0011] Preferably, the diisocyanate includes one or more of isophorone diisocyanate, 1,6-hexane diisocyanate, terephthalic diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate and phenyldimethyl diisocyanate.

[0012] The diol includes one or more of polycarbonate diol and polytetramethylene ether diol;

[0013] The first catalyst comprises dibutyltin dilaurate or stannous octoate.

[0014] Preferably, the molar ratio of the diisocyanate to the diol is 2:1; the mass of the first catalyst is 0.01 to 0.03 wt% of the total mass of the diisocyanate and the diol.

[0015] Preferably, the temperature of the first polymerization reaction is 70–100°C; and the time of the first polymerization reaction is 2–4 hours.

[0016] Preferably, the molar ratio of the diisocyanate to the difunctional aminobiphenyl is 10:2 to 3.5; and the molar ratio of the diisocyanate to the trifunctional aminophenylamine is 10:1 to 2.

[0017] The bifunctional aminobiphenyl includes one or more of 2,2'-bis(trifluoromethyl)diaminobiphenyl, 3,3'-dichloro-4,4'-diaminodiphenylmethane, isobutyl 3,5-diamino-p-chlorobenzoate, and diethyltoluenediamine; the trifunctional aminophenylamine includes one or more of tris(4-aminophenyl)amine, glycerol, triethanolamine, and triisopropanolamine.

[0018] Preferably, the temperature of the second polymerization reaction is 60–100°C; and the time of the second polymerization reaction is 6–12 hours.

[0019] Preferably, the acid anhydride includes one or more of 4,4'-(hexafluoroisopropene) phthalic anhydride, benzophenone dianhydride, pyromellitic dianhydride, diphenyl ether dianhydride, and biphenyl dianhydride;

[0020] The second catalyst comprises N,N-dimethylcyclohexylamine and N-methylaniline; the mass ratio of N,N-dimethylcyclohexylamine to N-methylaniline is 2:1 to 3.

[0021] Preferably, the molar ratio of 4,4'-diisocyanate-3,3'-dimethylbiphenyl to acid anhydride is 9-11:10.5; the mass of the second catalyst is 0.01-0.03 wt% of the total mass of 4,4'-diisocyanate-3,3'-dimethylbiphenyl and acid anhydride.

[0022] Preferably, the temperature of the third polymerization reaction is 130–160°C; and the time of the third polymerization reaction is 10–24 hours.

[0023] Preferably, the temperature of the fourth polymerization reaction is 60–100°C; and the time of the fourth polymerization reaction is 24–60 hours.

[0024] This invention provides a solvent-free method for preparing cross-linked PI-PUU polyfluorinated block copolymers. The invention uses solution polymerization to prepare cross-linked polyimide (PI)-polyurethane urea (PUU) polyfluorinated block copolymers. The solvent-free method is advantageous for various material processing and molding processes. Starting from relatively simple and readily available raw materials, this invention eliminates the need for intermediate separation and stringent imidization processes, directly obtaining the polyimide-polyurethane copolymer. Because both the soft and hard segments of the copolymer contain a certain amount of fluorine atoms, the cross-linked PI-PUU polyfluorinated block copolymer exhibits excellent water resistance and a low coefficient of friction. Attached Figure Description

[0025] Figure 1 It has the molecular chain structure of a cross-linked PI-PUU polyfluorinated block copolymer;

[0026] Figure 2The infrared spectrum of the cross-linked PI-PUU polyfluorinated block copolymer prepared in Example 1;

[0027] Figure 3 The stress-strain curves of the cross-linked PI-PUU polyfluorinated block copolymers prepared in Examples 1-3 are shown.

[0028] Figure 4 The stress-strain curves of TFT-3 before and after immersion in water for one week are shown. Detailed Implementation

[0029] This invention provides a solvent-free method for preparing cross-linked PI-PUU polyfluorinated block copolymers, comprising the following steps:

[0030] Diisocyanate, diol and first catalyst are mixed and subjected to first polymerization reaction to obtain polyurethane prepolymer;

[0031] The polyurethane prepolymer, bifunctional aminobiphenyl and trifunctional aminophenylamine are mixed and subjected to a second polymerization reaction to obtain hyperbranched amino-terminated PUU molecular chains.

[0032] 4,4'-diisocyanate-3,3'-dimethylbiphenyl, acid anhydride, and a second catalyst were mixed and subjected to a third polymerization reaction to obtain linear isocyanate-terminated PI molecular chains.

[0033] The hyperbranched amino-terminated PUU molecular chains and the linear isocyanate-terminated PI molecular chains are mixed and subjected to a fourth polymerization reaction to obtain a cross-linked PI-PUU polyfluorinated block copolymer.

[0034] This invention involves mixing a diisocyanate, a diol, and a first catalyst to conduct a first polymerization reaction, yielding a polyurethane prepolymer. In this invention, the diisocyanate preferably includes one or more of isophorone diisocyanate (IPDI), 1,6-hexanediisocyanate, terephthalic diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, and phenylenediamine diisocyanate. In this invention, the diol preferably includes one or more of polycarbonate diol (PCDL) and polytetramethylene ether diol. In this invention, the number average molecular weight of the diol is preferably 1000-5000, more preferably 2000. In this invention, the diol is preferably dehydrated before use. In this invention, the first catalyst preferably includes dibutyltin dilaurate (DBTDL) or stannous octoate.

[0035] In this invention, the molar ratio of the diisocyanate to the diol is preferably 2:1. In this invention, the mass of the first catalyst is preferably 0.01 to 0.03 wt% of the total mass of the diisocyanate and diol, more preferably 0.01 wt%.

[0036] In this invention, the temperature of the first polymerization reaction is preferably 70–100°C, more preferably 80–90°C; the time of the first polymerization reaction is preferably 2–4 hours, more preferably 2.5–3 hours. In this invention, the first polymerization reaction is preferably carried out under oil bath conditions. In this invention, the atmosphere of the first polymerization reaction is preferably a nitrogen atmosphere.

[0037] After obtaining the polyurethane prepolymer, the present invention mixes the polyurethane prepolymer, difunctional aminobiphenyl, and trifunctional aminophenylamine, and carries out a second polymerization reaction to obtain hyperbranched amino-terminated PUU molecular chains. In the present invention, the molar ratio of the diisocyanate to the difunctional aminobiphenyl is preferably 10:2 to 3.5, more preferably 10:2.5 to 3.1; the molar ratio of the diisocyanate to the trifunctional aminophenylamine is preferably 10:1 to 2, more preferably 10:1.5 to 1.8.

[0038] In this invention, the bifunctional aminobiphenyl preferably includes one or more of 2,2'-bis(trifluoromethyl)diaminobiphenyl (TFDB), 3,3'-dichloro-4,4'-diaminodiphenylmethane (MOCA), isobutyl 3,5-diamino-p-chlorobenzoate, and diethyltoluenediamine; the trifunctional aminophenylamine preferably includes one or more of tris(4-aminophenyl)amine (TAA), glycerol, triethanolamine, and triisopropanolamine.

[0039] In this invention, the preferred method of mixing the polyurethane prepolymer, bifunctional aminobiphenyl, and trifunctional aminophenylamine involves sequentially adding bifunctional aminobiphenyl and trifunctional aminophenylamine to the polyurethane prepolymer. This feeding sequence ensures appropriate branch lengths in the hyperbranched segments.

[0040] In this invention, the temperature of the second polymerization reaction is preferably 60–100°C, more preferably 80–90°C; the time of the second polymerization reaction is preferably 6–12 hours, more preferably 8–10 hours. In this invention, the second polymerization reaction is preferably carried out under oil bath conditions. In this invention, the atmosphere of the second polymerization reaction is preferably a nitrogen atmosphere.

[0041] In a specific embodiment of the present invention, after the first polymerization reaction is completed, a mixture of bifunctional aminobiphenyl and trifunctional aminophenylamine is directly added to the reaction system containing polyurethane prepolymer to carry out a second polymerization reaction, thereby obtaining hyperbranched amino-terminated PUU molecular chains.

[0042] This invention involves mixing 4,4'-diisocyanate-3,3'-dimethylbiphenyl (TODI), an anhydride, and a second catalyst to conduct a third polymerization reaction, yielding a linear isocyanate-terminated PI molecular chain. In this invention, the anhydride preferably comprises one or more of 4,4'-(hexafluoroisopropene)phthalic anhydride (6FDA), benzophenone dianhydride, pyromellitic dianhydride, diphenyl ether dianhydride, and biphenyl dianhydride. In this invention, the second catalyst preferably comprises N,N-dimethylcyclohexylamine (DMCA) and N-methylaniline (NMA); the mass ratio of N,N-dimethylcyclohexylamine to N-methylaniline is preferably 2:1 to 3, more preferably 1:1.

[0043] In this invention, the molar ratio of 4,4'-diisocyanate-3,3'-dimethylbiphenyl to the acid anhydride is 9–11:10.5, more preferably 9.5–10.25:10.5. In this invention, the mass of the second catalyst is preferably 0.01–0.03 wt% of the total mass of 4,4'-diisocyanate-3,3'-dimethylbiphenyl and the acid anhydride, more preferably 0.01 wt%.

[0044] In this invention, the mixing of 4,4'-diisocyanate-3,3'-dimethylbiphenyl (TODI), the acid anhydride, and the second catalyst preferably comprises: first heating and stirring 4,4'-diisocyanate-3,3'-dimethylbiphenyl (TODI) and the acid anhydride, and then adding the second catalyst. In this invention, the heating and stirring temperature is preferably 100–130°C, more preferably 110–120°C; the heating and stirring time is preferably 5–20 min, more preferably 10–15 min. In this invention, the mixing is preferably carried out under a nitrogen atmosphere.

[0045] In this invention, the temperature of the third polymerization reaction is preferably 130–160°C, more preferably 140–150°C; the time of the third polymerization reaction is preferably 10–24 hours, more preferably 12–20 hours. In this invention, the atmosphere of the third polymerization reaction is preferably a nitrogen atmosphere.

[0046] After obtaining hyperbranched amino-terminated PUU molecular chains and linear isocyanate-terminated PI molecular chains, this invention mixes the hyperbranched amino-terminated PUU molecular chains and linear isocyanate-terminated PI molecular chains and performs a fourth polymerization reaction to obtain a cross-linked PI-PUU polyfluorinated block copolymer. In this invention, the hyperbranched amino-terminated PUU molecular chains are used as soft segments, and the linear isocyanate-terminated PI molecular chains are used as hard segments, and the cross-linked PI-PUU polyfluorinated block copolymer is obtained through polymerization.

[0047] In this invention, the temperature of the fourth polymerization reaction is preferably 60–100°C, more preferably 80–90°C; the time of the fourth polymerization reaction is preferably 24–60 hours, more preferably 30–48 hours. In this invention, the fourth polymerization reaction is preferably carried out under oil bath conditions. In this invention, the atmosphere of the fourth polymerization reaction is preferably a nitrogen atmosphere.

[0048] In a specific embodiment of the present invention, after the second and third polymerization reactions are completed, the reaction system containing hyperbranched amino-terminated PUU molecular chains and the reaction system containing linear isocyanate-terminated PI molecular chains are directly mixed to carry out a fourth polymerization reaction to obtain a cross-linked PI-PUU polyfluorinated block copolymer.

[0049] In this invention, the PI content of the cross-linked PI-PUU polyfluorinated block copolymer is preferably 1 to 99 wt%, more preferably 15 to 40 wt%, and even more preferably 18.7 to 34.8 wt%.

[0050] In specific embodiments of the present invention, no separation or purification is performed during the preparation of the cross-linked PI-PUU polyfluorinated block copolymer.

[0051] The technical solutions of this invention will be clearly and completely described below with reference to the embodiments thereof. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0052] The structural formula of the raw materials used in the examples is as follows:

[0053]

[0054] The sources of the raw materials used are shown in Table 1.

[0055] Table 1 Sources of raw materials

[0056]

[0057]

[0058] Example 1

[0059] Sample name: TFT-1. PI content: 18.7 wt%.

[0060] (1) Synthesis of hyperbranched amino-terminated PUU molecular chains:

[0061] 2.245 g of IPDI was added to 10 g of PCDL, and 0.01 wt% of DBTDL was added as a catalyst. The mixture was reacted for 2.5 hours in an oil bath at 80 °C under nitrogen protection.

[0062] 1.021 g of TFDB and 0.421 g of TAA were added to the above solution in sequence, and the reaction was continued at 80 °C for 10 hours to obtain a reaction system containing hyperbranched amino-terminated PUU molecular chains.

[0063] (2) Synthesis of linear isocyanate-terminated PI molecular chains:

[0064] 1.907 g of 6FDA was added to 1.214 g of TODI under nitrogen protection. After stirring at 120 °C for 10 minutes, 0.01 wt% of a mixture of N,N-dimethylcyclohexylamine (DMCA) and N-methylaniline (NMA) (DMCA to NMA mass ratio of 1:1) was added as a catalyst. The temperature was then raised to 150 °C and the reaction was carried out for 12 hours to obtain a reaction system containing linear isocyanate-terminated PI molecular chains.

[0065] (3) The reaction system containing hyperbranched amino-terminated PUU molecular chains is blended with the reaction system containing linear isocyanate-terminated PI molecular chains and reacted in an oil bath at 90°C and under nitrogen protection for 48 hours to obtain a cross-linked PI-PUU polyfluorinated block copolymer, denoted as TFT-1.

[0066] Example 2

[0067] Sample name: TFT-2. PI content: 27.6 wt%.

[0068] (1) Synthesis of hyperbranched amino-terminated PUU molecular chains:

[0069] 2.245 g of IPDI was added to 10 g of PCDL, and 0.01 wt% of DBTDL was added as a catalyst. The mixture was reacted for 2.5 hours in an oil bath at 80 °C under nitrogen protection.

[0070] 1.021 g of TFDB and 0.449 g of TAA were added to the above solution in sequence, and the reaction was continued at 80 °C for 10 hours to obtain a reaction system containing hyperbranched amino-terminated PUU molecular chains.

[0071] (2) Synthesis of linear isocyanate-terminated PI molecular chains:

[0072] 3.186 g of 6FDA was added to 2.043 g of TODI under nitrogen protection. After stirring at 120 °C for 10 minutes, 0.01 wt% of a mixture of N,N-dimethylcyclohexylamine (DMCA) and N-methylaniline (NMA) (DMCA to NMA mass ratio of 1:1) was added as a catalyst. The temperature was then raised to 150 °C and the reaction was carried out for 12 hours to obtain a reaction system containing linear isocyanate-terminated PI molecular chains.

[0073] (3) The reaction system containing hyperbranched amino-terminated PUU molecular chains is blended with the reaction system containing linear isocyanate-terminated PI molecular chains and reacted in an oil bath at 90°C and under nitrogen protection for 48 hours to obtain a cross-linked PI-PUU polyfluorinated block copolymer, denoted as TFT-2.

[0074] Example 3

[0075] Sample name: TFT-3. PI content: 34.8 wt%.

[0076] (1) Synthesis of hyperbranched amino-terminated PUU molecular chains:

[0077] 2.245 g of IPDI was added to 10 g of PCDL, and 0.01 wt% of DBTDL was added as a catalyst. The mixture was reacted for 2.5 hours in an oil bath at 80 °C under nitrogen protection.

[0078] 1.021 g of TFDB and 0.469 g of TAA were added to the above solution in sequence, and the reaction was continued at 80 °C for 10 hours to obtain a reaction system containing hyperbranched amino-terminated PUU molecular chains.

[0079] (2) Synthesis of linear isocyanate-terminated PI molecular chains:

[0080] 4.487 g of 6FDA was added to 2.861 g of TODI under nitrogen protection. After stirring at 120 °C for 10 minutes, 0.01 wt% of a mixture of N,N-dimethylcyclohexylamine (DMCA) and N-methylaniline (NMA) (DMCA to NMA mass ratio of 1:1) was added as a catalyst. The temperature was then raised to 150 °C and the reaction was carried out for 12 hours to obtain a reaction system containing linear isocyanate-terminated PI molecular chains.

[0081] (3) The reaction system containing hyperbranched amino-terminated PUU molecular chains is blended with the reaction system containing linear isocyanate-terminated PI molecular chains and reacted in an oil bath at 90°C and under nitrogen protection for 48 hours to obtain a cross-linked PI-PUU polyfluorinated block copolymer, denoted as TFT-3.

[0082] Comparative Example 1

[0083] Sample Name: PUU

[0084] (1) Add 2.245g of IPDI to 10g of PCDL and add 0.01wt% of DBTDL as a catalyst. React for 2.5 hours in an oil bath at 80℃ under nitrogen protection.

[0085] (2) 1.021g of TFDB and 0.367g of TAA were added to the above solution one after another, and the reaction was continued at 80℃ for 10 hours to obtain PUU.

[0086] Comparative Example 2

[0087] Sample name: PI

[0088] 4.487 g of 6FDA was added to 2.697 g of TODI under nitrogen protection. After stirring at 120 °C for 10 minutes, 0.01 wt% of a mixture of N,N-dimethylcyclohexylamine (DMCA) and N-methylaniline (NMA) (DMCA to NMA in a mass ratio of 1:1) was added as a catalyst. The temperature was then raised to 150 °C and the reaction was carried out for 12 hours to obtain PI.

[0089] Test case

[0090] (1) Figure 1 The molecular chain structure is that of a cross-linked PI-PUU polyfluorinated block copolymer. Figure 1 The wavy line in the lower left corner could represent either PI or PUU. Figure 1 It can be seen that the PI-PUU polyfluorinated block polymer is a hyperbranched network structure with trifunctional groups as crosslinking points and PI or PUU chains as branches.

[0091] (2) Figure 2 The infrared spectrum of the cross-linked PI-PUU polyfluorinated block copolymer prepared in Example 1 is shown at 2261 cm⁻¹. -1 The absence of a characteristic NCO peak indicates that the isocyanate group has reacted completely. (3373.27 cm⁻¹) -1 The characteristic NH peak is visible at 1600-1750 cm⁻¹. -1 The peak corresponds to the -C=O stretching vibration peak of the urea group and carbamate in PUU. 1781 cm⁻¹ -1 The peak at this point corresponds to the -C=O stretching vibration of the imine group, indicating the presence of imine bonds in the PI chain segment. In conclusion, the PI-PUU polyfluorinated block copolymer was successfully prepared.

[0092] (3) Figure 3 The stress-strain curves of the crosslinked PI-PUU polyfluorinated block copolymers prepared in Examples 1-3 are shown below. Figure 3It can be seen that as the PI content increases, the elongation at break of the material decreases, but the fracture strength increases, indicating that the strength and toughness of the material can be controlled by adjusting the PI content.

[0093] (4) The performance comparison of the examples and comparative examples is shown in Table 2. The friction coefficient of Comparative Example 1 exceeds the range of the friction testing machine (>1). The test standards for fracture strength and elongation at break in Table 2 are GB / T1040.1-2018; the test standards for friction coefficient and wear rate are GB / T 3960-1983.

[0094] Table 2 Performance Comparison of Examples and Comparative Examples

[0095]

[0096]

[0097] As shown in Table 2, the embodiments combine the tensile properties of both PUU and PI materials. More importantly, the friction-reducing and wear-resistant properties of the materials are significantly enhanced compared to the comparative examples.

[0098] (5) Figure 4 The stress-strain curves of TFT-3 before and after immersion in water for one week are shown below. Figure 4 It can be seen that the tensile properties of the example did not change significantly before and after immersion in water for one week, indicating that the cross-linked PI-PUU polyfluorinated block copolymer prepared in this invention has good water resistance.

[0099] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A solvent-free method for preparing cross-linked PI-PUU polyfluorinated block copolymers, comprising the following steps: Diisocyanate, diol and first catalyst are mixed and subjected to first polymerization reaction to obtain polyurethane prepolymer; The polyurethane prepolymer, bifunctional aminobiphenyl, and trifunctional aminophenylamine are mixed and subjected to a second polymerization reaction to obtain hyperbranched amino-terminated PUU molecular chains; the bifunctional aminobiphenyl includes 2,2'-bis(trifluoromethyl)diaminobiphenyl. 4,4'-diisocyanate-3,3'-dimethylbiphenyl, an anhydride, and a second catalyst are mixed and subjected to a third polymerization reaction to obtain linear isocyanate-terminated PI molecular chains; the anhydride includes 4,4'-(hexafluoroisopropene)phthalic anhydride. The hyperbranched amino-terminated PUU molecular chains and the linear isocyanate-terminated PI molecular chains are mixed and subjected to a fourth polymerization reaction to obtain a cross-linked PI-PUU polyfluorinated block copolymer.

2. The method according to claim 1, characterized in that, The diisocyanate includes one or more of isophorone diisocyanate, 1,6-hexane diisocyanate, terephthalic diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate and phenyldimethyl diisocyanate. The diol includes one or more of polycarbonate diol and polytetramethylene ether diol; The first catalyst comprises dibutyltin dilaurate or stannous octoate.

3. The method according to claim 1 or 2, characterized in that, The molar ratio of the diisocyanate to the diol is 2:1; the mass of the first catalyst is 0.01~0.03 wt% of the total mass of the diisocyanate and the diol.

4. The method according to claim 1, characterized in that, The temperature of the first polymerization reaction is 70~100℃; the time of the first polymerization reaction is 2~4 hours.

5. The method according to claim 1, characterized in that, The molar ratio of the diisocyanate to the difunctional aminobiphenyl is 10:2 to 3.5; the molar ratio of the diisocyanate to the trifunctional aminophenylamine is 10:1 to 2. The trifunctional aminophenylamines include tris(4-aminophenyl)amine.

6. The method according to claim 1 or 5, characterized in that, The temperature of the second polymerization reaction is 60~100℃; the time of the second polymerization reaction is 6~12 hours.

7. The method according to claim 1, characterized in that, The second catalyst comprises N,N-dimethylcyclohexylamine and N-methylaniline; the mass ratio of N,N-dimethylcyclohexylamine to N-methylaniline is 2:1~3.

8. The method according to claim 1 or 7, characterized in that, The mass of the second catalyst is 0.01 to 0.03 wt% of the total mass of 4,4'-diisocyanate-3,3'-dimethylbiphenyl and acid anhydride.

9. The method according to claim 1, characterized in that, The temperature of the third polymerization reaction is 130~160℃; the time of the third polymerization reaction is 10~24 hours.

10. The method according to claim 1, characterized in that, The temperature of the fourth polymerization reaction is 60~100℃; the time of the fourth polymerization reaction is 24~60 hours.

Citation Information

Patent Citations

  • All-solid-state lithium-ion battery based on topological-structured polymer electrolyte

    CN105762403A

  • Aqueous polyorganosiloxane hybrid resin dispersion

    IN201934004553A