Polyacrylonitrile-based carbon fibers, graphitized carbon fibers, and methods of making and using the same
By introducing a carbonization pretreatment step between low-temperature carbonization and high-temperature carbonization, the nitrogen-carbon ratio of the carbon fiber structure can be controlled, thus solving the problem of poor carbon fiber performance in the prior art and realizing the preparation of high-performance carbon fibers.
Patent Information
- Application Number
- CN202211323497.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-27
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-10-27
AI Technical Summary
The lack of effective control over the internal structure of carbon fibers during the denitrification process in the high-temperature carbonization stage in existing technologies leads to poor carbon fiber performance.
By introducing a carbonization pretreatment step between low-temperature and high-temperature carbonization, the nitrogen-to-carbon ratio R of the carbon fiber structure is controlled to be ≤3.5, thereby optimizing the orderliness of the carbon fiber and preparing high-performance carbon fibers.
The mechanical properties of carbon fiber have been improved, especially the tensile strength and modulus of graphitized carbon fiber, which exceed the M46J level of Toray Industries, Inc. of Japan.
Smart Images

Figure CN117987965B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of carbon fiber technology, and more specifically, to polyacrylonitrile-based carbon fibers, graphitized carbon fibers, their preparation methods, and applications. Background Technology
[0002] Polyacrylonitrile-based carbon fiber is a high-performance material prepared through polymerization, spinning, and oxidation carbonization processes, primarily using acrylonitrile monomers. During the oxidation process, the long, straight polyacrylonitrile molecular chains within the polyacrylonitrile precursor gradually form a "trapezoidal" polymer structure with excellent heat resistance. In the subsequent carbonization process, non-carbon elements are gradually released by releasing small molecule gases to form graphite sheets during high-temperature carbonization, thus perfecting the internal structure of the fiber and improving the final macroscopic mechanical properties of the carbon fiber.
[0003] During the high-temperature carbonization stage, fibers that have undergone low-temperature carbonization still need further removal of non-carbon elements, such as denitrification. Below 1000℃, denitrification primarily involves the removal of NH3 and HCN, causing a rapid decrease in nitrogen content. Releasing a single molecule of NH3 only reduces nitrogen content and does not affect carbon content; in other words, this method of removing non-carbon elements does not reduce the final carbon yield of the carbon fiber. However, if the fiber removes nitrogen by releasing a single molecule of HCN, then both the nitrogen content and the final carbon yield of the carbon fiber will decrease. The third method of nitrogen removal is N2, with a peak denitrification temperature of approximately 1300℃. This mainly involves solid-phase condensation polymerization, enriching carbon elements and generating a six-membered carbon network planar structure, which eventually evolves into the disordered graphite structure of carbon fibers. Summary of the Invention
[0004] The inventors discovered in their research that denitrification during the high-temperature carbonization stage has a significant impact on the amorphous structure (mainly amorphous carbon, as well as some carbon-nitrogen-containing structures) and ordered region structure (graphite-like structure) inside carbon fibers, and seriously affects the performance of high-performance carbon fibers. However, there is a lack of research in this area in the existing technology.
[0005] The inventors conducted an in-depth study on the structural evolution mechanism of the carbonization process in the preparation of polyacrylonitrile-based carbon fibers, and proposed the nitrogen-carbon ratio of the carbon fiber structure as an intermediate control index. By controlling this index, the structural order of the carbon fiber can be controlled, thereby obtaining high-performance carbon fibers. A corresponding processing method suitable for controlling this index was proposed, namely, adding a brief carbonization pretreatment between the low-temperature carbonization step and the high-temperature carbonization step. This method has been successfully applied to the preparation process of high-modulus polyacrylonitrile carbon fibers.
[0006] To solve the above-mentioned technical problems in the prior art, the present invention provides a polyacrylonitrile-based carbon fiber, a graphitized carbon fiber, and preparation methods and applications thereof. The present invention improves the mechanical properties of carbon fibers by controlling the structure of polyacrylonitrile-based carbon fibers and improving corresponding preparation methods.
[0007] One of the objectives of the present invention is to provide a polyacrylonitrile-based carbon fiber, wherein the structural nitrogen-to-carbon ratio R of the polyacrylonitrile-based carbon fiber satisfies 0<R≤3.5;
[0008] The structural nitrogen-to-carbon ratio R=(A D +A N ) / A G ;
[0009] wherein, A N is the product of the Y-axis coordinate corresponding to the spectral peak of the N peak in the Raman spectrum test curve and the half-peak width of the N peak;
[0010] A D is the product of the Y-axis coordinate corresponding to the spectral peak of the D peak in the Raman spectrum test curve and the half-peak width of the D peak;
[0011] A G is the product of the Y-axis coordinate corresponding to the spectral peak of the G peak in the Raman spectrum test curve and the half-peak width of the G peak.
[0012] In the Raman spectrum of the present invention, A N mainly refers to nitrogen-containing structures, the A G peak mainly refers to sp 2 hybridized carbon atom structures; the A D peak refers to sp 3 hybridized carbon atom structures; through empirical summary, the present invention derives the formula for the above structural nitrogen-to-carbon ratio R=(A D +A N ) / A G ; the R value calculated by this formula can effectively reflect the structural order of the polyacrylonitrile-based carbon fiber, and can be used as an indicator to judge the mechanical properties of the graphitized carbon fiber prepared by graphitizing the polyacrylonitrile-based carbon fiber.
[0013] The inventors of the present application have found through research that when the structural nitrogen-to-carbon ratio R of the polyacrylonitrile-based carbon fiber is ≤3.5, it indicates that the carbon fiber has a regular internal arrangement and a large amount of ordered carbon structures (mainly sp2 hybridized carbon atoms), and does not form many structural defects, resulting in good mechanical properties of the final carbon fiber; when R>3.5, it indicates that the carbon fiber has a high nitrogen content, leading to a large amount of amorphous structures inside the carbon fiber. When the structural nitrogen-to-carbon ratio R of the polyacrylonitrile-based carbon fiber of the present invention satisfies 0<R≤3.5, the structural order of the polyacrylonitrile-based carbon fiber is high, and the corresponding prepared graphitized carbon fiber has better mechanical properties.
[0014] In the polyacrylonitrile-based carbon fiber of the present invention, preferably,
[0015] The structure has a nitrogen-to-carbon ratio of 0. <R≤3.25。
[0016] In the polyacrylonitrile-based carbon fiber of the present invention, preferably,
[0017] The A N The corresponding spectral peaks have Raman shift coordinates ranging from 1500 to 1540 cm⁻¹. -1 The preferred height is 1510–1530 cm. -1 ;
[0018] A D The corresponding spectral peaks have Raman shift coordinates ranging from 1320 to 1380 cm⁻¹. -1 The preferred height is 1355-1370cm. -1 ;
[0019] A G The X-axis coordinates corresponding to the spectral peaks are 1575–1620 cm. -1 The preferred height is 1590–1620 cm. -1 .
[0020] In the polyacrylonitrile-based carbon fiber of the present invention, preferably,
[0021] The laser wavelength range used in Raman spectroscopy testing is 510–640 nm; and / or,
[0022] The laser power is 5–15 mW; and / or,
[0023] The cumulative exposure time ranges from 1 to 20 seconds; and / or,
[0024] The cumulative number of exposures is 1 to 5; and / or,
[0025] During testing, the laser power output rate was 50-100%.
[0026] The second objective of this invention is to provide a method for preparing polyacrylonitrile-based carbon fibers, comprising the following steps:
[0027] In the preparation of polyacrylonitrile-based carbon fibers, a carbonization pretreatment step is added between low-temperature carbonization treatment and high-temperature carbonization treatment.
[0028] Preferably used for preparing the polyacrylonitrile-based carbon fiber as described in one of the objectives of this invention.
[0029] In the preparation method of polyacrylonitrile-based carbon fiber described in this invention, preferably,
[0030] The carbonization pretreatment temperature is higher than the high-temperature carbonization treatment temperature; and / or,
[0031] The carbonization pretreatment time is shorter than the high-temperature carbonization treatment time.
[0032] Preferably,
[0033] The carbonization pretreatment temperature is 1400–1700℃; preferably 1550–1700℃; for example, it can be 1400℃, 1450℃, 1500℃, 1550℃, 1600℃, 1650℃, 1700℃, and / or,
[0034] The carbonization pretreatment time is 10–20 seconds; preferably 10–15 seconds; for example, it can be 10 seconds, 10 seconds, 11 seconds, 12 seconds, 13 seconds, 14 seconds, 15 seconds, 16 seconds, 17 seconds, 18 seconds, 19 seconds, or 20 seconds; and / or,
[0035] The processing atmosphere is an inert atmosphere, preferably nitrogen; and / or,
[0036] There is no draw ratio during the carbonization pretreatment process, i.e., the draw ratio is 0.
[0037] In the preparation method of polyacrylonitrile-based carbon fiber described in this invention, preferably,
[0038] Prior to the low-temperature carbonization treatment, a pre-oxidation treatment of the precursor fiber is also included;
[0039] Preferably,
[0040] The precursor fiber is a polyacrylonitrile precursor fiber; and / or,
[0041] In this invention, conventional conditions can be used for the pre-oxidation treatment. Preferably, the highest temperature of the pre-oxidation treatment does not exceed 280°C, the lowest temperature is not lower than 170°C, the total pre-oxidation time does not exceed 120 min, the treatment atmosphere is air, and the draw ratio is 0-6%; preferably 0-3%; more preferably, a six-stage pre-oxidation treatment is used.
[0042] More preferably,
[0043] Polyacrylonitrile precursor fibers are produced by wet spinning or dry-jet wet spinning; and / or,
[0044] The polyacrylonitrile precursor fiber is at 3–24 K.
[0045] In the present invention, the draw ratio refers to: the ratio of the linear velocity of the furnace exit roller to the linear velocity of the furnace entrance roller, denoted as λ, and the ratio of the difference between λ and 1 to 1, and the corresponding value is the draw ratio. That is, for example, when λ>1.00, it is called positive drafting, and when λ<1.00, it is called negative drafting. For example, when λ=1.01, it is 1% positive drafting; when λ=0.99, it is 1% negative drafting or -1% drafting.
[0046] In the preparation method of the polyacrylonitrile-based carbon fiber according to the present invention,
[0047] the temperature of the low-temperature carbonization treatment is 300 to 800°C; and / or,
[0048] the total time of the low-temperature carbonization treatment is 2 to 6 min; and / or,
[0049] the draw ratio is 0 to 6%; and / or,
[0050] the treatment atmosphere is an inert atmosphere, preferably nitrogen.
[0051] More preferably, the low-temperature carbonization treatment is carried out in four stages, low-carbon four-stage, the first stage: 300 to 400°C, the second stage 400 to 500°C, the third stage 550 to 650°C, and the fourth stage 650 to 800°C, and the treatment time of each stage is 30 to 50 seconds (preferably 40 seconds).
[0052] In the preparation method of the polyacrylonitrile-based carbon fiber according to the present invention, preferably,
[0053] the temperature of the high-temperature carbonization treatment is 1000 to 1400°C; and / or,
[0054] the total time of the high-temperature carbonization treatment is 1 to 3 min; and / or,
[0055] the draw ratio is -4 to -1%; and / or,
[0056] the treatment atmosphere is an inert atmosphere, preferably nitrogen.
[0057] The present invention performs pre-oxidation, low-temperature carbonization, and high-temperature carbonization treatment on polyacrylonitrile precursors, and sets a special carbonization pretreatment step between low-temperature carbonization and high-temperature carbonization, which can regulate a reasonable range of structural nitrogen-carbon ratio of carbon fibers. The structural nitrogen-carbon ratio of the polyacrylonitrile-based carbon fiber of the present invention is 0<R≤3.5. The polyacrylonitrile-based carbon fiber with a structural nitrogen-carbon ratio of 0<R≤3.5 according to the present invention is subjected to subsequent graphitization treatment at a higher heat treatment temperature, and a high-modulus polyacrylonitrile-based graphitized carbon fiber can be prepared.
[0058] When polyacrylonitrile-based carbon fibers are prepared without using the method described in this invention, including the specific carbonization pretreatment step, and the nitrogen-to-carbon ratio R > 3.5, it indicates a relatively high nitrogen content in the carbon fibers. This results in a greater presence of amorphous structures within the carbon fibers. This is because the low-temperature carbonized fibers did not undergo the carbonization pretreatment step of this invention; instead, the nitrogen was not released as completely as possible during the high-temperature carbonization process, leaving more air bubbles or pores inside the fibers, leading to poor mechanical properties in the final carbon fibers. When such carbon fibers undergo graphitization at even higher temperatures, the final graphitized carbon fibers will also exhibit poor mechanical properties.
[0059] A third objective of this invention is to provide the application of the polyacrylonitrile-based carbon fiber described in one objective of this invention or the polyacrylonitrile-based carbon fiber prepared by the preparation method described in another objective of this invention in the preparation of graphitized carbon fiber.
[0060] The fourth objective of this invention is to provide a method for preparing graphitized carbon fibers, comprising the following steps:
[0061] The polyacrylonitrile-based carbon fiber is graphitized to obtain the graphitized carbon fiber. Preferably, the polyacrylonitrile-based carbon fiber is the polyacrylonitrile-based carbon fiber described in one of the objectives of this invention or the polyacrylonitrile-based carbon fiber prepared by the preparation method described in another objective of this invention.
[0062] In the method for preparing graphitized carbon fibers according to the present invention, preferably,
[0063] The graphitization treatment temperature is 2200–2500℃; and / or,
[0064] The graphitization treatment time is 1–5 min; and / or,
[0065] The draw ratio is 5–10%; and / or,
[0066] The processing atmosphere is an inert atmosphere, preferably argon.
[0067] The fifth objective of this invention is to provide a graphitized carbon fiber prepared by the preparation method described in the fourth objective of this invention, preferably,
[0068] The graphitized carbon fiber has a tensile strength ≥4000 MPa, preferably ≥4288 MPa; and / or,
[0069] The tensile modulus is ≥448 GPa, preferably ≥455 GPa.
[0070] The sixth objective of this invention is to provide the application of graphitized carbon fibers prepared by the preparation method described in the fourth objective of this invention or graphitized carbon fibers described in the fifth objective of this invention in high-strength materials.
[0071] In this invention, the high-strength material is a common high-strength material in the prior art, such as composite materials for aerospace vehicles, lightweight materials for automobiles, and propeller composite materials for wind turbine generators.
[0072] The endpoints and any values of the ranges disclosed in this invention are not limited to the precise ranges or values; these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein. In the following, various technical solutions can, in principle, be combined with each other to obtain new technical solutions, which should also be considered as specifically disclosed herein.
[0073] Compared with the prior art, the present invention has at least the following advantages:
[0074] This invention also proposes a parameter model for the nitrogen-carbon ratio of carbon fiber structure, which can reasonably quantify the internal structure of carbon fiber. This parameter can be well applied to the preparation of high-modulus polyacrylonitrile-based carbon fiber, guiding the production and preparation work for the control index in the preparation process of high-performance carbon fiber.
[0075] This invention introduces a carbonization pretreatment step between the low-temperature carbonization and high-temperature carbonization steps. The high-temperature instantaneous treatment during the carbonization pretreatment stage rapidly denitrifies the carbon fibers after low-temperature carbonization, thereby allowing for better control of the nitrogen-to-carbon ratio in the polyacrylonitrile-based carbon fibers. This can be used to obtain polyacrylonitrile-based graphitized carbon fibers with good mechanical properties, or to prepare high-modulus carbon fibers, which has significant guiding significance for the high-performance carbon fiber industry. Therefore, the carbonization pretreatment proposed in this invention significantly improves the mechanical properties of the final graphitized carbon fibers.
[0076] The mechanical properties of the graphitized carbon fibers prepared by this invention exceed those of Toray Industries' M46J grade. Attached Figure Description
[0077] Figure 1 The image shows the Raman spectral curve of the polyacrylonitrile-based carbon fiber in Example 1 of this invention.
[0078] The horizontal axis represents the Raman displacement (cm). -1 The vertical axis represents the Raman intensity (AU); Y D The peak of the D peak in the Raman spectral test curve; Y N The spectral peak of the N peak in the Raman spectral test curve; Y G The spectral peak of the G peak in the Raman spectroscopy test curve; FWHM D The full width at half maximum (FWHM) of peak D in the Raman spectroscopy test curve; GThe full width at half maximum (FWHM) of the G peak in the Raman spectroscopy test curve; N This represents the full width at half maximum (FWHM) of the N peak in the Raman spectroscopy test curve. Detailed Implementation
[0079] The present invention will now be described in detail with reference to the accompanying drawings and embodiments. It should be noted that the following embodiments are only used to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the content of the present invention are still within the scope of protection of the present invention.
[0080] It should also be noted that the various specific technical features described in the following embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the various possible combinations will not be described separately in this invention.
[0081] Furthermore, various embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention. The resulting technical solutions are part of the original disclosure of this specification and also fall within the protection scope of the present invention.
[0082] Unless otherwise specified, the raw materials used in the examples and comparative examples are all disclosed in the prior art, such as those that can be directly purchased or prepared according to the preparation methods disclosed in the prior art.
[0083] Test method:
[0084] The mechanical properties of carbon fiber bundles were tested according to the national standard GB / T25749-2011.
[0085] The Raman spectroscopy test curves were obtained by fitting using LabVIEW software.
[0086]
Example 1
[0087] Polyacrylonitrile precursor fibers produced using domestically produced 3K wet-spun yarns underwent a gradient-heating pre-oxidation treatment in air. The pre-oxidation process consisted of six stages at temperatures of 170℃, 220℃, 235℃, 253℃, 258℃, and 263℃, with a total pre-oxidation time of 80 min, each stage lasting 13.3 min, and a traction ratio of 0. The pre-oxidized polyacrylonitrile fibers were then subjected to low-temperature carbonization, carbonization pretreatment, and high-temperature carbonization in high-purity nitrogen to obtain polyacrylonitrile-based carbon fibers. The low-temperature carbonization stage involved a gradient temperature increase, employing four stages: 300℃, 450℃, 550℃, and 750℃, with each stage lasting 40 seconds and a traction ratio of 0. The carbonization pretreatment was performed at 1400℃ for 15 seconds, with a traction ratio of 0. The high-temperature carbonization process employed a four-stage heating process: 1000℃ in the first stage, 1150℃ in the second stage, 1280℃ in the third stage, and 1400℃ in the fourth stage. The high-temperature carbonization time was 2 minutes, with each stage lasting 30 seconds. The draw ratio was -4%, resulting in polyacrylonitrile-based carbon fibers.
[0088] Raman spectroscopy of polyacrylonitrile-based carbon fibers after high-temperature carbonization was performed using a Raman spectrometer manufactured by Horiba Jobin Yvon, France. The results are as follows: Figure 1 As shown; the Raman laser was 533 nm, the laser power was 10 mW, the exposure time was 10 s, the cumulative exposure times were 5, and the output power was 50%; then the A values of the D peak, N peak, and G peak of its Raman spectrum were obtained respectively. N A D and A G Finally, substitute it into the calculation formula: R = (A D +A N ) / A G The nitrogen-to-carbon ratio of the polyacrylonitrile-based carbon fiber was determined. The carbon fiber was then subjected to a higher-temperature graphitization treatment at 2400℃ for 90 seconds, with a draw ratio of 5%. The mechanical properties of the carbon fiber bundles were tested according to the national standard GB / T25749-2011, and the test results are shown in Table 1.
[0089]
Example 2
[0090] A carbonization pretreatment was performed between low-temperature carbonization and high-temperature carbonization, with a temperature of 1450℃ and a residence time of 15s. Other operating steps and process parameters were the same as in Example 1. The mechanical properties of the carbon fiber bundles were tested according to the national standard GB / T25749-2011, and the test results are shown in Table 1.
[0091]
Example 3
[0092] A carbonization pretreatment was performed between low-temperature carbonization and high-temperature carbonization, with a temperature of 1500℃ and a residence time of 15s. Other operating steps and process parameters were the same as in Example 1. The mechanical properties of the carbon fiber bundles were tested according to the national standard GB / T25749-2011, and the test results are shown in Table 1.
[0093]
Example 4
[0094] A carbonization pretreatment was performed between low-temperature carbonization and high-temperature carbonization, with a temperature of 1550℃ and a residence time of 15s. Other operating steps and process parameters were the same as in Example 1. The mechanical properties of the carbon fiber bundles were tested according to the national standard GB / T25749-2011, and the test results are shown in Table 1.
[0095]
Example 5
[0096] A carbonization pretreatment was performed between low-temperature carbonization and high-temperature carbonization, with a temperature of 1600℃ and a residence time of 15s. Other operating steps and process parameters were the same as in Example 1. The mechanical properties of the carbon fiber bundles were tested according to the national standard GB / T25749-2011, and the test results are shown in Table 1.
[0097]
Example 6
[0098] A carbonization pretreatment was performed between low-temperature carbonization and high-temperature carbonization, with a temperature of 1650℃ and a residence time of 15s. Other operating steps and process parameters were the same as in Example 1. The mechanical properties of the carbon fiber bundles were tested according to the national standard GB / T25749-2011, and the test results are shown in Table 1.
[0099]
Example 7
[0100] A carbonization pretreatment was performed between low-temperature carbonization and high-temperature carbonization, with a temperature of 1700℃ and a residence time of 15s. Other operating steps and process parameters were the same as in Example 1. The mechanical properties of the carbon fiber bundles were tested according to the national standard GB / T25749-2011, and the test results are shown in Table 1.
[0101]
Example 8
[0102] A carbonization pretreatment was performed between low-temperature carbonization and high-temperature carbonization, with a temperature of 1450℃ and a residence time of 20s. Other operating steps and process parameters were the same as in Example 1. The mechanical properties of the carbon fiber bundles were tested according to the national standard GB / T25749-2011, and the test results are shown in Table 1.
[0103]
Example 9
[0104] A carbonization pretreatment was performed between low-temperature carbonization and high-temperature carbonization, with a temperature of 1500℃ and a residence time of 20s. Other operating steps and process parameters were the same as in Example 1. The mechanical properties of the carbon fiber bundles were tested according to the national standard GB / T25749-2011, and the test results are shown in Table 1.
[0105]
Example 10
[0106] A carbonization pretreatment was performed between low-temperature carbonization and high-temperature carbonization, with a temperature of 1550℃ and a residence time of 20s. Other operating steps and process parameters were the same as in Example 1. The mechanical properties of the carbon fiber bundles were tested according to the national standard GB / T25749-2011, and the test results are shown in Table 1.
[0107]
Example 11
[0108] A carbonization pretreatment was performed between low-temperature carbonization and high-temperature carbonization, with a temperature of 1600℃ and a residence time of 20s. Other operating steps and process parameters were the same as in Example 1. The mechanical properties of the carbon fiber bundles were tested according to the national standard GB / T25749-2011, and the test results are shown in Table 1.
[0109]
Example 12
[0110] A carbonization pretreatment was performed between low-temperature carbonization and high-temperature carbonization, with a temperature of 1650℃ and a residence time of 20s. Other operating steps and process parameters were the same as in Example 1. The mechanical properties of the carbon fiber bundles were tested according to the national standard GB / T25749-2011, and the test results are shown in Table 1.
[0111]
Example 13
[0112] A carbonization pretreatment was performed between low-temperature carbonization and high-temperature carbonization, with a temperature of 1700℃ and a residence time of 20s. Other operating steps and process parameters were the same as in Example 1. The mechanical properties of the carbon fiber bundles were tested according to the national standard GB / T25749-2011, and the test results are shown in Table 1.
[0113]
Example 14
[0114] A carbonization pretreatment was performed between low-temperature carbonization and high-temperature carbonization, with a temperature of 1700°C and a residence time of 10 seconds. Other operating steps and process parameters were the same as in Example 1.
[0115]
Comparative Example 1
[0116] The preparation conditions are the same as in Example 1, except that the carbonization pretreatment step is not included.
[0117] Raman spectrometers manufactured by Horiba Jobin Yvon, France, were used to perform Raman spectroscopy on fibers that had undergone high-temperature carbonization. The Raman laser was 533 nm, with a power of 10 mW, an exposure time of 10 s, a cumulative exposure count of 5, and an output power of 50%. The A values of the D, N, and G peaks were then obtained. N A D and A G Finally, substitute it into the calculation formula: R = (A D +A N ) / A G The nitrogen-to-carbon ratio of the polyacrylonitrile-based carbon fiber was determined. The carbon fiber was then subjected to a higher-temperature graphitization treatment at 2400℃ for 90 seconds, with a draw ratio of 5%. The mechanical properties of the carbon fiber bundles were tested according to the national standard GB / T25749-2011, and the test results are shown in Table 1.
[0118] [Comparative Example 2]
[0119] The laser power for the Raman test was 40mW, the output power was 100%, the exposure time was 60s, and the cumulative exposure count was 10. Other operating procedures and process parameters were the same as in Comparative Example 1, but the correct Raman data could not be obtained. This is because the full-power output in Comparative Example 2 resulted in high laser intensity, which easily ablated the carbon fiber surface, altering the physical properties of the sample test points, thus failing to obtain the correct Raman data. The mechanical properties of the carbon fiber bundles were tested according to the national standard GB / T25749-2011, and the test results are shown in Table 1.
[0120] [Comparative Example 3]
[0121] A carbonization pretreatment was performed between low-temperature carbonization and high-temperature carbonization, with a temperature of 1000℃ and a residence time of 2 seconds. Other operating steps and process parameters were the same as in Example 1. The mechanical properties of the carbon fiber bundles were tested according to the national standard GB / T25749-2011, and the test results are shown in Table 1.
[0122] [Comparative Example 4]
[0123] A carbonization pretreatment was performed between low-temperature carbonization and high-temperature carbonization, with a temperature of 1700°C and a residence time of 30 seconds. Other operating steps and process parameters were the same as in Example 1.
[0124] Comparative Example 4 failed to collect samples, therefore no specific data on the mechanical properties of the carbon fiber and the value of the nitrogen-carbon ratio R of the carbon fiber structure are available.
[0125] The nitrogen-to-carbon ratio R of the polyacrylonitrile carbon fibers obtained in the above comparative examples and embodiments, and the results of the final mechanical properties (including tensile strength and tensile modulus) of the polyacrylonitrile-based graphitized carbon fibers are listed in Table 1.
[0126] Table 1
[0127]
[0128]
[0129] In this invention, a smaller structural nitrogen-to-carbon ratio R indicates fewer defects in the carbon fiber, resulting in higher tensile strength (MPa) and tensile modulus (GPa), meaning better mechanical properties of the prepared graphitized carbon fiber. As can be seen from Example 1 and Comparative Example 1, Example 1, by adding a carbonization pretreatment step compared to Comparative Example 1, significantly increases the tensile strength and tensile modulus of the prepared graphitized carbon fiber, resulting in better mechanical properties.
[0130] The present invention has been described in detail above with reference to specific embodiments and exemplary examples; however, these descriptions should not be construed as limiting the present invention. Those skilled in the art will understand that various equivalent substitutions, modifications, or improvements can be made to the technical solutions and embodiments of the present invention without departing from the spirit and scope of the invention, and all such modifications and improvements fall within the scope of the present invention. The scope of protection of the present invention is defined by the appended claims.
Claims
1. A polyacrylonitrile-based carbon fiber, wherein the polyacrylonitrile-based carbon fiber has a nitrogen-to-carbon ratio R of 0. <R≤3.5; The structure has a nitrogen-to-carbon ratio R =( A D +A N ) / A G ;in, A N It is the product of the Y-axis coordinate corresponding to the N-peak of the Raman spectrum test curve and the half-width of the N-peak. A D It is the product of the Y-axis coordinate corresponding to the D peak of the Raman spectrum test curve and the full width at half maximum (FWHM) of the D peak. A G It is the product of the Y-axis coordinate corresponding to the G peak of the Raman spectrum test curve and the full width at half maximum (FWHM) of the G peak; A N The corresponding spectral peaks have Raman shift coordinates ranging from 1500 to 1540 cm⁻¹. -1 The spectral peaks of the Raman characteristic peaks of the segment; A D The corresponding spectral peaks have Raman shift coordinates ranging from 1320 to 1380 cm⁻¹. -1 The spectral peaks of the Raman characteristic peaks of the segment; A G The corresponding spectral peaks have Raman shift coordinates ranging from 1575 to 1620 cm⁻¹. -1 The spectral peaks of the Raman characteristic peaks of the segment; The lasers used in Raman spectroscopy testing had a wavelength range of 510–640 nm, a power range of 5–15 mW, a cumulative exposure time range of 1–20 s, a cumulative exposure count range of 1–5, and a laser power output rate of 50–100%. When preparing polyacrylonitrile-based carbon fibers, a carbonization pretreatment step is added between low-temperature carbonization and high-temperature carbonization. The carbonization pretreatment temperature is 1400~1700℃; the carbonization pretreatment time is 10~20 seconds; the treatment atmosphere is an inert atmosphere; and the draw ratio is 0 during the carbonization pretreatment process.
2. The polyacrylonitrile-based carbon fiber according to claim 1, characterized in that: The structure has a nitrogen-to-carbon ratio of 0. <R≤3.2。 3. The polyacrylonitrile-based carbon fiber according to claim 1, characterized in that: The A N The corresponding spectral peaks have Raman shift coordinates ranging from 1510 to 1530 cm⁻¹. -1 The spectral peaks of the Raman characteristic peaks of the segment; A D The corresponding spectral peaks have Raman shift coordinates ranging from 1355 to 1370 cm⁻¹. -1 The spectral peaks of the Raman characteristic peaks of the segment; A G The corresponding spectral peaks have Raman shift coordinates ranging from 1590 to 1620 cm⁻¹. -1 The spectral peaks of the Raman characteristic peaks of the segment.
4. A method for preparing polyacrylonitrile-based carbon fiber, comprising the following steps: In the preparation of polyacrylonitrile-based carbon fibers, a carbonization pretreatment step is added between low-temperature carbonization treatment and high-temperature carbonization treatment. The carbonization pretreatment temperature is 1400~1700℃; the carbonization pretreatment time is 10~20 seconds; the treatment atmosphere is an inert atmosphere; and the stretching ratio during the carbonization pretreatment is 0. Used to prepare polyacrylonitrile-based carbon fibers according to any one of claims 1-3.
5. The method for preparing polyacrylonitrile-based carbon fiber according to claim 4, characterized in that: The carbonization pretreatment temperature is 1550~1700℃; and / or, The carbonization pretreatment time is 10-15 seconds.
6. The method for preparing polyacrylonitrile-based carbon fiber according to claim 4, characterized in that: Prior to the low-temperature carbonization process, a pre-oxidation treatment of the precursor fiber is also included.
7. The method for preparing polyacrylonitrile-based carbon fiber according to claim 6, characterized in that: The precursor fiber is a polyacrylonitrile precursor fiber; and / or, The pre-oxidation treatment temperature is 170~280℃, the total pre-oxidation time does not exceed 120min, the treatment atmosphere is air, and the draw ratio is 0~6%.
8. The method for preparing polyacrylonitrile-based carbon fiber according to claim 7, characterized in that: The draw ratio of the pre-oxidation treatment is 0~3%.
9. The method for preparing polyacrylonitrile-based carbon fiber according to claim 7, characterized in that: Polyacrylonitrile precursor fibers are produced by wet spinning or dry-jet wet spinning; and / or, The polyacrylonitrile precursor fiber is at 3~24K.
10. The method for preparing polyacrylonitrile-based carbon fiber according to claim 4, characterized in that: The low-temperature carbonization treatment is performed at a temperature of 300~800℃; and / or, The total time for low-temperature carbonization treatment is 2-6 minutes; and / or, The draw ratio for low-temperature carbonization treatment is 0-6%; and / or, The processing atmosphere for low-temperature carbonization is an inert atmosphere.
11. The method for preparing polyacrylonitrile-based carbon fiber according to claim 4, characterized in that: The high-temperature carbonization treatment is carried out at a temperature of 1000~1400℃; and / or, The total time for high-temperature carbonization treatment is 1~3 min; and / or, The draw ratio for high-temperature carbonization treatment is -4 to -1%; and / or, The processing atmosphere for high-temperature carbonization is an inert atmosphere.
12. The application of a polyacrylonitrile-based carbon fiber according to any one of claims 1-3 or a polyacrylonitrile-based carbon fiber prepared by any one of claims 4-11 in the preparation of graphitized carbon fibers.
13. A method for preparing graphitized carbon fibers, comprising the following steps: The polyacrylonitrile-based carbon fiber is graphitized to obtain the graphitized carbon fiber. The polyacrylonitrile-based carbon fiber is prepared by the polyacrylonitrile-based carbon fiber according to any one of claims 1-3 or by the preparation method according to any one of claims 4-11.
14. The method for preparing graphitized carbon fiber according to claim 13, characterized in that: The graphitization treatment temperature is 2200~2500℃; and / or, The graphitization treatment time is 1~5 min; and / or, The draw ratio for graphitization treatment is 5-10%; and / or, The graphitization process is carried out in an inert atmosphere.
Citation Information
Patent Citations
High-tensile strength high-tensile modulus carbon fiber and preparation method thereof
CN109023592A