Catalysts, processes for their preparation and use, cyclic lactones, processes for their preparation
By using the prepared carbon-based catalyst M@C, cyclic lactones can be synthesized from cyclic ketones using air as an oxygen source. This solves the problem of low efficiency in the existing air oxidation method and achieves efficient, low-cost and environmentally friendly lactone production.
Patent Information
- Application Number
- CN202211341018.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-30
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-10-30
AI Technical Summary
In the existing technology, the preparation of lactones using the peroxy acid oxidation method has serious equipment corrosion, complicated operation, serious pollution and safety hazards. The hydrogen peroxide oxidation method has low utilization rate, while the air oxidation method requires a high-efficiency catalyst to improve oxidation efficiency.
A carbon-based catalyst M@C was prepared using a metal-organic framework synthesized from inorganic ions and organic ligands as a precursor. This catalyst was used to catalyze the synthesis of cyclic lactones from cyclic ketones, utilizing air as an oxygen source. The catalyst exhibited high selectivity and a large specific surface area.
It achieves highly efficient catalytic reactions using air as an oxygen source, reduces production costs, and produces almost no byproducts, thereby improving the conversion rate of cyclic ketones and the selectivity of lactones.
Smart Images

Figure CN118002123B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalytic synthesis technology, specifically to a catalyst, its preparation method and application, and cyclic lactones and their preparation methods. Background Technology
[0002] Polyesters, due to their permeability, thermoplasticity, and biocompatibility, are widely used in the production of environmentally friendly materials, human tissue scaffolds, medical carriers, surgical sutures, and other products. Polyesters possess enormous market value; reportedly, total polyester production capacity was approximately 47 million tons in 2015 and approximately 63.975 million tons in 2020, representing an average annual growth rate of 6.18%. It is projected that production capacity will reach 75 million tons by 2023. Cyclic lactones are an important raw material used in the production of polyesters.
[0003] Low molecular weight cyclic lactones are colorless, volatile aromatic liquids, while high molecular weight cyclic lactones are colorless, odorless, waxy solids. Cyclic lactones are mainly used in the synthesis of polyesters, copolymerization with lipids, and resin modification. They can improve the physical properties of copolymers and enhance the light transmittance, gloss, and anti-stick properties of resins. Therefore, organic cyclic lactones have enormous application potential and a broad market prospect.
[0004] Currently, the Baeyer-Villiger oxidation reaction is mainly used to synthesize organic cyclic lactones. This reaction is one of the hot topics in organic chemistry research. Scholars are constantly conducting in-depth research and development of new catalysts suitable for the Baeyer-Villiger oxidation reaction in order to improve the catalytic performance of the catalysts.
[0005] In 1899, Baeyer and Villiger et al. first reported a reaction in which sodium persulfate, prepared from sodium sulfate and concentrated sulfuric acid, was used as an oxidant, followed by further oxidation of menthone to prepare lactones. Subsequent researchers expanded upon this research, discovering numerous cyclic ketones that could be oxidized to lactones by peroxy acids, and based on this, they deduced the reaction mechanism. This type of reaction was named the Baeyer-Villiger oxidative rearrangement. Depending on the type of oxidant, the main synthetic methods can currently be categorized into peroxy acid oxidation, enzymatic oxidation, hydrogen peroxide oxidation, and oxygen (air) oxidation.
[0006] Industrially, the peroxy acid oxidation method is commonly used to produce lactones. However, this process suffers from problems such as severe equipment corrosion caused by peroxy acid, complex operation, serious pollution, and safety hazards. Few domestic enterprises are able to use this method to prepare lactones (Lu Qiaosen et al., Research progress on caprolactone production process [J] Modern Chemical Industry 2015, 35(2):36-39). Compared with the peroxy acid oxidation method, the hydrogen peroxide oxidation method uses hydrogen peroxide as an oxidant to directly oxidize the substrate cyclic ketone, which simplifies the reaction process, is environmentally friendly, and reduces safety hazards. However, the oxidizing power of hydrogen peroxide is relatively weak, requiring the use of excess hydrogen peroxide in the reaction. The ineffective decomposition of some hydrogen peroxide results in a low utilization rate of hydrogen peroxide, and the excess water in the reaction system can cause hydrolysis of the lactone.
[0007] Theoretically, cyclic ketones can be completely converted into lactones using oxygen (air) oxidation, which meets the requirements of modern green chemical production. Furthermore, oxygen (air) oxidation has high efficiency, high lactone yield, and safer production, making it a method of significant research value. CN102603447A and CN102702152A demonstrate the catalytic oxidation of cyclic ketones using oxygen as the oxygen source, achieving high lactone yields. Compared to oxygen, air is cheaper and more readily available. However, when using air as the oxygen source, its relatively weak oxidizing power makes the oxidation reaction difficult to carry out without a catalyst. Therefore, using air as the oxygen source requires the design and development of highly efficient catalysts. Summary of the Invention
[0008] The purpose of this invention is to overcome the aforementioned technical problems in the prior art and provide a catalyst, its preparation method and application, and a cyclic lactone and its preparation method. The carbon-based catalyst prepared using a metal-organic framework synthesized from inorganic ions and organic ligands as a precursor not only possesses a large specific surface area but also has a tunable pore structure. This catalyst exhibits high conversion rates for various cyclic ketones, high selectivity for the generated lactones, and is easily recyclable after the reaction. When applied to the synthesis of cyclic lactones from cyclic ketones, the reaction can be carried out using air as an oxygen source, significantly reducing production costs; furthermore, this catalyst exhibits good selectivity, with almost no byproducts generated during the catalytic reaction.
[0009] To achieve the above objectives, the first aspect of the present invention provides a catalyst, characterized in that:
[0010] The catalyst is designated M@C or MO. x @C;
[0011] Wherein, x is 0.5-1.5, the loading of M is 25-62 wt%, M is selected from Cu or Fe, and the specific surface area of the catalyst is 20-120 m². 2 / g.
[0012] A second aspect of the present invention provides a method for preparing a catalyst, characterized in that the method comprises the following steps:
[0013] (1) Mix the metal precursor, organic ligand and first solvent, and dissolve them to obtain a reaction solution;
[0014] (2) The reaction solution is subjected to a hydrothermal reaction to obtain the reaction product;
[0015] (3) The reaction product is separated by solid-liquid separation to obtain the MOF precursor;
[0016] (4) The MOF precursor is calcined to obtain a catalyst;
[0017] The active metal element in the catalyst is Cu or Fe;
[0018] The molar ratio of the metal precursor, the organic ligand, and the first solvent is 1:0.3-1.0:20-100.
[0019] A third aspect of the present invention provides a catalyst prepared by the above method.
[0020] The fourth aspect of this invention provides the application of the catalyst described in the first or third aspect in the catalytic synthesis of cyclic lactones from cyclic ketones.
[0021] The fifth aspect of the present invention provides a method for synthesizing cyclic lactones from cyclic ketones, characterized in that,
[0022] A catalytic reaction is carried out in the presence of a cyclic ketone, a first oxidant, a second solvent, a second oxidant, and a catalyst to yield a cyclic lactone.
[0023] The catalyst is selected from the catalysts described in the first or third aspect.
[0024] The sixth aspect of the present invention provides a cyclic lactone obtained by the method described in the fifth aspect.
[0025] Through the above technical solutions, the catalyst, its preparation method and application, and the cyclic lactone and its preparation method provided by the present invention achieve the following beneficial effects:
[0026] Carbon-based catalysts prepared using metal-organic frameworks synthesized from inorganic ions and organic ligands as precursors not only possess a large specific surface area but also have tunable pore structures. When applied to the synthesis of cyclic lactones from cyclic ketones, the reaction can proceed using air as the oxygen source, significantly reducing production costs. Furthermore, this catalyst exhibits good selectivity, with virtually no byproducts generated during the catalytic reaction. Attached Figure Description
[0027] Figure 1 TEM image of the catalyst prepared in Example 3;
[0028] Figure 2 Aberration-corrected electron micrograph of the catalyst prepared in Example 3;
[0029] Figure 3 The BET test results are for the catalyst prepared in Example 3;
[0030] Figure 4 This is a TEM image of the catalyst prepared in Example 3. Detailed Implementation
[0031] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0032] To achieve the above objectives, the first aspect of the present invention provides a catalyst, characterized in that:
[0033] The catalyst is designated M@C or MO. x @C, where x is 0.5-1.5, the loading of M is 25-62 wt%, M is selected from Cu or Fe, and the specific surface area of the catalyst is 20-120 m². 2 / g.
[0034] In this invention, the specific surface area of the catalyst meets the above-mentioned range, which can improve the catalytic efficiency of the catalyst. By synergistically selecting Cu or Fe as the active metal component, the catalyst can have high catalytic activity.
[0035] According to the present invention, the loading of M is 33-43 wt%.
[0036] Furthermore, the catalyst has a specific surface area of 70-120 m². 2 / g.
[0037] According to the present invention, the catalyst has an average pore size of 1-50 nm.
[0038] Furthermore, the catalyst has an average pore size of 10-40 nm.
[0039] According to the present invention, the dispersion of the catalyst is 80-100%, preferably 90-100%.
[0040] According to the present invention, the catalyst is a single-atom catalyst.
[0041] A second aspect of the present invention provides a method for preparing a catalyst, characterized in that the method comprises the following steps:
[0042] (1) Mix the metal precursor, organic ligand and first solvent, and dissolve them to obtain a reaction solution;
[0043] (2) The reaction solution is subjected to a hydrothermal reaction to obtain the reaction product;
[0044] (3) The reaction product is separated by solid-liquid separation to obtain the MOF precursor;
[0045] (4) The MOF precursor is calcined to obtain a catalyst;
[0046] The active metal element in the catalyst is Cu or Fe;
[0047] The molar ratio of the metal precursor, the organic ligand, and the first solvent is 1:0.3-1:20-100.
[0048] In this invention, the metal precursor, organic ligand and first solvent are used in the above molar ratio, and the prepared MOF precursor has a stable structure and high catalytic performance after calcination.
[0049] According to the present invention, the molar ratio of the metal precursor, the organic ligand and the first solvent is 1:0.3-0.8:35-80.
[0050] In this invention, the metal precursor is selected from copper salts or iron salts.
[0051] In this invention, the copper salt is selected from at least one of CuCl2·nH2O, CuNO3·nH2O and CuSO4·nH2O, wherein n≥0.
[0052] In this invention, the iron salt is selected from at least one of FeCl3·nH2O, Fe(NO3)3·nH2O and Fe2(SO4)3·nH2O, wherein n≥0.
[0053] According to the present invention, the organic ligand is selected from carboxylic acid compounds having the R-(COOH)n structure, wherein R is a C6-C17 hydrocarbon group and n is an integer from 1 to 4.
[0054] In this invention, the organic ligands with the above-described structure can interact with metal precursors to form stable MOF structures.
[0055] Furthermore, the organic ligand is selected from at least one of terephthalic acid, 1,3,5-pyromellitic acid, 1,2,4-phenyltricarboxylic acid, 3,3',5,5'-biphenyltetracarboxylic acid, and oleic acid.
[0056] According to the present invention, the first solvent is selected from at least one of methanol, anhydrous ethanol, n-butanol and N,N-dimethylformamide.
[0057] In this invention, the first solvent described above is used to fully disperse the organic ligand and the metal precursor.
[0058] According to the present invention, the temperature of the hydrothermal reaction is 120-180°C.
[0059] Furthermore, the temperature of the hydrothermal reaction is 130-160℃.
[0060] According to the present invention, the hydrothermal reaction time is 4-24 hours.
[0061] Furthermore, the hydrothermal reaction time is 6-18 hours.
[0062] According to the present invention, a protective roasting gas is introduced during the roasting process.
[0063] In this invention, the protective roasting gas is selected from nitrogen and / or argon.
[0064] According to the present invention, the calcination temperature is 400-1000℃.
[0065] Furthermore, the calcination temperature is 500-800℃.
[0066] According to the present invention, the roasting time is 3-6 hours.
[0067] According to the present invention, the heating rate of the calcination is 2-10℃ / min.
[0068] In this invention, the above-mentioned calcination conditions are beneficial to the crystallization of the active component, thereby improving the catalytic activity of the catalyst.
[0069] A third aspect of the present invention provides a catalyst prepared by the above method.
[0070] According to the present invention, the catalyst is a single-atom catalyst.
[0071] In this invention, the specific surface area, average pore size, dispersion and loading of the catalyst are consistent with those of the catalyst provided in the first aspect of this invention, and will not be described again.
[0072] The fourth aspect of this invention provides the application of the catalyst described in the first or third aspect in the catalytic synthesis of cyclic lactones from cyclic ketones.
[0073] The fifth aspect of the present invention provides a method for synthesizing cyclic lactones from cyclic ketones, characterized in that,
[0074] A catalytic reaction is carried out in the presence of a cyclic ketone, a first oxidant, a second solvent, a second oxidant, and a catalyst to yield a cyclic lactone.
[0075] The catalyst is selected from the catalysts described in the first or third aspect.
[0076] According to the present invention, the mass ratio of the cyclic ketone, the first oxidant and the second solvent is 1:1-4:10-40:0.05-0.3.
[0077] In this invention, the mass ratio of the cyclic ketone, the first oxidant, and the second solvent is within the above-mentioned range, resulting in high catalytic performance. Further catalysts meeting the above-mentioned range can improve the conversion rate of cyclic ketones while saving costs.
[0078] Furthermore, the mass ratio of the cyclic ketone, the first oxidant, and the second solvent is 1:1.5-3:15-30:0.08-0.2.
[0079] According to the present invention, the cyclic ketone is selected from at least one of cyclopentanone, 2-methylcyclohexanone, cyclohexanone, 4-methylcyclohexanone, and 4-ethylcyclohexanone.
[0080] According to the present invention, the first oxidant is selected from at least one of benzaldehyde, p-methylbenzaldehyde, isobutyraldehyde and n-butyraldehyde.
[0081] According to the present invention, the second solvent is selected from at least one of acetonitrile, ethyl acetate and 1,2-dichloroethane.
[0082] In this invention, the use of the solvents described above is beneficial for the full dispersion of each substance in the system.
[0083] According to the present invention, the second oxidant is selected from an oxygen-containing gas, and the concentration of oxygen in the second oxidant is 10-30% by volume.
[0084] Furthermore, the second oxidant is air.
[0085] According to the present invention, the flow rate of the second oxidant is 10-40 mL / min, preferably 20-40 mL / min.
[0086] According to the present invention, the temperature of the catalytic reaction is 30-60°C, preferably 40-50°C.
[0087] According to the present invention, the catalytic reaction time is 6-12 hours, preferably 8-10 hours.
[0088] The sixth aspect of the present invention provides a cyclic lactone obtained by the method described in the fifth aspect.
[0089] In the following embodiments, unless otherwise specified, all raw materials used are commercially available.
[0090] The following are the test methods for performance parameters involved in this invention:
[0091] (1) Conversion rate:
[0092]
[0093] (2) Yield:
[0094]
[0095] (3) BET test: The instrument model is BELSORP-MAX, the specific surface area is calculated by the Brunauer-Emmett-Teller (BET) equation, and the pore size distribution is analyzed by the Barrett-Joyner-Halenda (BJH) test method. 0.1g of sample was degassed and pretreated at 120℃ for 4h, and then adsorption-desorption test was performed by passing N2 at -196℃.
[0096] (4) Dispersion test: The test instrument was a fully automated adsorption analyzer from MICROMERITICS (ASAP2020M+C). 0.5g of catalyst was weighed, and a vacuum was drawn to a degree of 10. -4 Pa, then H2 is introduced, and the temperature is raised to 240℃. Reduction is performed at this temperature for 4 hours. Then, a vacuum is drawn to achieve a vacuum level of 1.33 × 10⁻⁶. -4 Pa, then the H2 adsorption isotherm curve was measured at 150℃, and then a vacuum was drawn to achieve a vacuum degree of 1.33×10. -4 Pa, repeat the H2 adsorption isotherm measurement.
[0097]
[0098] Where V H Where W is the volume of H2 consumed, W is the mass of the catalyst, P is the mass fraction of M in the catalyst, and M is the mass of the catalyst. M M is the relative molecular mass;
[0099] The catalyst loading was determined by ICP method;
[0100] The composition of the catalyst was determined by XPS.
[0101] Example 1
[0102] (1) Mix 1.705g of copper chloride dihydrate, 0.498g of terephthalic acid (n is 2, R is C6 phenyl) and 14.62g of N,N-dimethylformamide, and sonicate at room temperature for 30min to obtain a reaction solution;
[0103] (2) The reaction solution was transferred to a hydrothermal reactor lined with polytetrafluoroethylene and reacted at 120°C for 4 hours. After the reaction was completed, the mixture was allowed to cool to room temperature naturally to obtain the reaction product.
[0104] (3) The reaction product was centrifuged, washed and dried to obtain 1.2 g of precursor;
[0105] (4) Place 1g of the precursor in a tube furnace and heat it to 1000℃ at 10℃ / min under a N2 atmosphere. Hold the temperature for 4h and allow it to cool naturally. Then grind it in an agate mortar to obtain 0.8g of CuO. 0.5 @C catalyst.
[0106] Example 2
[0107] (1) Mix 1.705 g of copper chloride dihydrate, 2.101 g of 1,3,5-pyromellitic acid (n is 3, R is C6 phenyl) and 32.04 g of methanol, and sonicate at room temperature for 30 min to obtain a reaction solution;
[0108] (2) The reaction solution was transferred to a hydrothermal reactor lined with polytetrafluoroethylene and reacted at 180°C for 24 hours. After the reaction was completed, the mixture was allowed to cool to room temperature naturally to obtain the reaction product.
[0109] (3) The reaction product was centrifuged, washed and dried to obtain 1g of precursor;
[0110] (4) Place 0.5g of the precursor in a tube furnace and heat it to 400℃ at 2℃ / min under a N2 atmosphere. Hold the temperature for 6 hours. After natural cooling, grind it in an agate mortar to obtain 0.35g of CuO. 0.5 @C catalyst.
[0111] Example 3
[0112] (1) Mix 0.853 g of copper chloride dihydrate, 0.424 g of oleic acid (n is 1, R is a C17 alkenyl group) and 18.53 g of n-butanol, and sonicate at room temperature for 30 min to obtain a reaction solution;
[0113] (2) The reaction solution was transferred to a hydrothermal reactor lined with polytetrafluoroethylene and reacted at 160°C for 12 hours. After the reaction was completed, the mixture was allowed to cool to room temperature naturally to obtain the reaction product.
[0114] (3) The reaction product was centrifuged, washed and dried to obtain 0.65 g of precursor;
[0115] (4) Place 0.1g of the precursor in a tube furnace, heat it to 800℃ at 5℃ / min under an Ar atmosphere and hold for 5h. After natural cooling, grind it in an agate mortar to obtain 0.2g of Cu@C catalyst.
[0116] Example 4
[0117] (1) Mix 1.364 g of copper chloride dihydrate, 0.841 g of 1,3,5-pyromellitic acid (n is 3, R is C6 phenyl) and 29.48 g of anhydrous ethanol, and sonicate at room temperature for 30 min to obtain a reaction solution.
[0118] (2) The reaction solution was transferred to a hydrothermal reactor lined with polytetrafluoroethylene and reacted at 150°C for 8 hours. After the reaction was completed, the mixture was allowed to cool to room temperature naturally to obtain the reaction product.
[0119] (3) The reaction product was centrifuged, washed and dried to obtain 1g of precursor;
[0120] (4) Place 0.5g of the precursor in a tube furnace, heat it to 700℃ at 5℃ / min under N2 atmosphere and hold for 4h. After natural cooling, grind it in an agate mortar to obtain 0.4g of Cu@C catalyst.
[0121] Example 5
[0122] (1) Mix 2.02g of ferric nitrate nonahydrate, 0.525g of 1,3,5-trimethylammoniazolic acid (n is 3, R is C6 phenyl) and 12.94g of N,N-dimethylformamide, and sonicate at room temperature for 30min to obtain a reaction solution;
[0123] (2) The reaction solution was transferred to a hydrothermal reactor lined with polytetrafluoroethylene and reacted at 130°C for 18 hours. After the reaction was completed, the temperature was allowed to drop to room temperature naturally to obtain the reaction product.
[0124] (3) The reaction product was centrifuged, washed and dried to obtain 1.09 g of precursor;
[0125] (4) Place 0.5g of the precursor in a tube furnace, heat it to 700℃ at 5℃ / min under N2 atmosphere and hold for 3h. After natural cooling, grind it in an agate mortar to obtain 0.3g of Fe@C catalyst.
[0126] Example 6
[0127] (1) Mix 7.998g of ferric sulfate, 3.362g of 1,2,4-benzenetricarboxylic acid (n is 3, R is C6 phenyl) and 55.28g of anhydrous ethanol, and sonicate at room temperature for 30min to obtain a reaction solution;
[0128] (2) The reaction solution was transferred to a hydrothermal reactor lined with polytetrafluoroethylene and reacted at 170°C for 18 hours. After the reaction was completed, the mixture was allowed to cool to room temperature naturally to obtain the reaction product.
[0129] (3) The reaction product was centrifuged, washed and dried to obtain 2.8 g of precursor;
[0130] (4) 1g of precursor was placed in a tube furnace and heated to 600℃ at 2℃ / min under Ar atmosphere and held for 5h. After natural cooling, it was ground in an agate mortar to obtain 0.82g of Fe@C catalyst.
[0131] Example 7
[0132] (1) Mix 5.406 g of ferric chloride hexahydrate, 1.982 g of 3,3',5,5'-biphenyltetracarboxylic acid (n is 4, R is C12 phenyl) and 51.26 g of methanol, and sonicate at room temperature for 30 min to obtain a reaction solution;
[0133] (2) The reaction solution was transferred to a hydrothermal reactor lined with polytetrafluoroethylene and reacted at 160°C for 12 hours. After the reaction was completed, the mixture was allowed to cool to room temperature naturally to obtain the reaction product.
[0134] (3) The reaction product was centrifuged, washed and dried to obtain 4.8 g of precursor;
[0135] (4) Place 1g of the precursor in a tube furnace and heat it to 600℃ at 2℃ / min under air atmosphere, hold it for 5h, and after natural cooling, grind it in an agate mortar to obtain 1.5g of FeO. 1.5 @C catalyst.
[0136] Example 8
[0137] (1) Mix 2.703 g of ferric chloride hexahydrate, 1.661 g of terephthalic acid (n is 2, R is C6 phenyl) and 37.06 g of n-butanol, and sonicate at room temperature for 30 min to obtain a reaction solution;
[0138] (2) The reaction solution was transferred to a hydrothermal reactor lined with polytetrafluoroethylene and reacted at 140°C for 24 hours. After the reaction was completed, the mixture was allowed to cool to room temperature naturally to obtain the reaction product.
[0139] (3) The reaction product was centrifuged, washed and dried to obtain 2.2 g of precursor;
[0140] (4) Place 0.5g of the precursor in a tube furnace, heat it to 1000℃ at 5℃ / min under an Ar atmosphere and hold for 6h. After natural cooling, grind it in an agate mortar to obtain 1.3g of FeO@C catalyst.
[0141] Example 9
[0142] (1) Mix 0.853 g of copper chloride dihydrate, 0.225 g of oleic acid (n is 1, R is C17 alkenyl) and 6.1 g of n-butanol, and sonicate at room temperature for 30 min to obtain a reaction solution;
[0143] (2) The reaction solution was transferred to a hydrothermal reactor lined with polytetrafluoroethylene and reacted at 160°C for 12 hours. After the reaction was completed, the mixture was allowed to cool to room temperature naturally to obtain the reaction product.
[0144] (3) The reaction product was centrifuged, washed and dried to obtain 0.5 g of precursor;
[0145] (4) Place 0.1g of the precursor in a tube furnace, heat it to 800℃ at 5℃ / min under an Ar atmosphere and hold for 5h. After natural cooling, grind it in an agate mortar to obtain 0.18g of Cu@C catalyst.
[0146] Example 10
[0147] (1) Mix 0.853 g of copper chloride dihydrate, 0.424 g of oleic acid (n is 1, R is C17 alkenyl) and 18.53 g of n-butanol, and sonicate at room temperature for 30 min to obtain a reaction solution;
[0148] (2) The reaction solution was transferred to a hydrothermal reactor lined with polytetrafluoroethylene and reacted at 100°C for 20 hours. After the reaction was completed, the mixture was allowed to cool to room temperature naturally to obtain the reaction product.
[0149] (3) The reaction product was centrifuged, washed and dried to obtain 0.5 g of precursor;
[0150] (4) Place 0.1g of the precursor in a tube furnace, heat it to 800℃ at 5℃ / min under an Ar atmosphere and hold for 5h. After natural cooling, grind it in an agate mortar to obtain 0.17g of Cu@C catalyst.
[0151] Comparative Example 1
[0152] Following the method of Example 1, except that the amount of terephthalic acid used was 1g, the rest was the same as in Example 1, yielding 0.8g of CuO. 0.5 @C catalyst.
[0153] Comparative Example 2
[0154] Following the method of Example 1, except that copper chloride dihydrate was replaced with an equimolar amount of magnesium nitrate, the rest was the same as in Example 1, yielding 0.8 g of MgO. 0.5 @C catalyst.
[0155] Application Example 1-10
[0156] Add 0.15 g of the catalyst prepared in Examples 1-10, 1 g of cyclohexanone, 2 g of benzaldehyde, and 30 g of 1,2-dichloroethane to a three-necked flask. Purge with air at a rate of 40 mL / min and react at 50 °C for 10 h.
[0157] The obtained product was filtered and the clear liquid was analyzed by gas chromatography. The conversion rate of cyclic ketones and the yield of cyclic lactones are shown in Table 2.
[0158] Application Example 11
[0159] The method was the same as in Application Example 3, except that 1 g of cyclopentanone, 3 g of isobutyraldehyde, and 15 g of acetonitrile were used. The rest was the same as in Application Example 1. The cyclic ketone conversion rate and the yield of the cyclic lactone are shown in Table 2.
[0160] Application Example 12
[0161] The method was the same as in Application Example 1, except that 1 g of cyclohexanone, 2 g of benzaldehyde, and 50 g of 1,2-dichloroethane were used. The rest of the process was identical to Application Example 1. The conversion rates of the cyclic ketones and the yields of the cyclic lactones are shown in Table 2.
[0162] Application Examples 13 and 14
[0163] The method was the same as in Application Example 1, except that the amount of catalyst used was 0.3 g and 0.5 g, respectively. Everything else was the same as in Application Example 1. The cyclic ketone conversion and cyclic lactone yield were measured and are shown in Table 2.
[0164] Application Example 15
[0165] The method was the same as in Application Example 1, except that the rate of air introduction was 10 mL / min. Everything else was the same as in Application Example 1. The cyclic ketone conversion and cyclic lactone yield were measured and are shown in Table 2.
[0166] Application Example 16
[0167] The method is the same as in Application Example 1, except that an oxygen-nitrogen mixture with a volume fraction of 10% is introduced at a rate of 40 mL / min.
[0168] Table 1
[0169]
[0170] Table 2
[0171]
[0172] As can be seen from Table 1, Examples 1-16 have good results, with a conversion rate of cyclic ketones of not less than 40% and a yield of cyclic lactones of not less than 32%.
[0173] Among them, the catalysts prepared in Examples 3-6 and Example 10, which satisfy the preferred technical solutions of the present invention, have the highest specific surface area. Changing their preparation conditions will reduce the specific surface area of the obtained catalysts to some extent. As can be seen from Table 2, Application Examples 3-6 and Application Examples 10-11 have the best conversion and yield, while changing the conditions so that the mass ratio of cyclic ketone: first oxidant: second solvent does not meet the range, and changing the flow rate of the second oxidant will significantly reduce the conversion and yield of the reaction.
[0174] Figure 1 It can be seen that the catalyst morphology is coated with carbon material. Figure 2 The spherical aberration characterization results show that single atoms were successfully synthesized. Figure 3 It can be seen that the catalyst pores are mainly mesopores, and the pore sizes are distributed in the range of 1-100 nm, with an average pore size of 1-50 nm.
[0175] pass Figure 4 The observation of Cu(111) and C(002) crystal lattice fringes proves that the sample successfully synthesized a single-atom catalyst.
[0176] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combining the various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A method for synthesizing cyclic lactones from cyclic ketones, characterized in that, A catalytic reaction is carried out in the presence of a cyclic ketone, a first oxidant, a second solvent, a second oxidant, and a catalyst to yield a cyclic lactone. The catalyst is denoted as M@C or MO. x @C; Wherein, x is 0.5-1.5, the loading of M is 25-43 wt%, and M is selected from Cu or Fe; the catalyst is a single-atom catalyst; the specific surface area of the catalyst is 20-120 m². 2 / g; The preparation method of the catalyst includes the following steps: (1) Mix the metal precursor, organic ligand and first solvent, and dissolve them to obtain a reaction solution; (2) The reaction solution is subjected to a hydrothermal reaction to obtain the reaction product; (3) The reaction product is subjected to solid-liquid separation to obtain the MOF precursor; (4) The MOF precursor is calcined to obtain a catalyst; wherein the active metal element in the catalyst is Cu or Fe; The molar ratio of the metal precursor, the organic ligand, and the first solvent is 1:0.3-1:20-100.
2. The method according to claim 1, characterized in that, The loading of M is 33-43 wt%; The catalyst has a specific surface area of 70-120 m². 2 / g; And / or, the average pore size of the catalyst is 1-50 nm; And / or, the dispersion of the catalyst is 80-100%.
3. The method according to claim 2, wherein, The catalyst has an average pore size of 10-40 nm; And / or, the dispersion of the catalyst is 90-100%.
4. The method according to claim 1, characterized in that, The molar ratio of the metal precursor, the organic ligand, and the first solvent is 1:0.3-0.8:35-80; And / or, the metal precursor is selected from copper salts or iron salts.
5. The method according to claim 4, characterized in that, The copper salt is selected from at least one of CuCl2·nH2O, CuNO3·nH2O and CuSO4·nH2O, wherein n≥0; And / or, the iron salt is selected from at least one of FeCl3·nH2O, Fe(NO3)3·nH2O and Fe2(SO4)3·nH2O, wherein n≥0.
6. The method according to any one of claims 1-5, characterized in that, The organic ligands are selected from those having R-(COOH) n Carboxylic acid compounds with a structure where R is a C6-C17 hydrocarbon group and n is an integer from 1 to 4; And / or, the first solvent is selected from at least one of methanol, anhydrous ethanol, n-butanol, and N,N-dimethylformamide.
7. The method according to any one of claims 1-5, characterized in that, The organic ligand is selected from at least one of terephthalic acid, 1,3,5-pyromellitic acid, 1,2,4-triphenylcarboxylic acid, 3,3',5,5'-biphenyltetracarboxylic acid, and oleic acid.
8. The method according to any one of claims 1-5, characterized in that, The temperature of the hydrothermal reaction is 120-180℃; And / or, the hydrothermal reaction time is 4-24 hours.
9. The method according to any one of claims 1-5, wherein, The hydrothermal reaction temperature is 130-160℃; And / or, the hydrothermal reaction time is 6-18 hours.
10. The method according to any one of claims 1-5, characterized in that, Protective roasting gas is introduced during the roasting process; And / or, the calcination temperature is 400-1000℃; And / or, the calcination time is 3-6 hours; And / or, the heating rate of the calcination is 2-10 °C / min.
11. The method according to any one of claims 1-5, wherein, The roasting temperature is 500-800℃.
12. The method according to any one of claims 1-5, characterized in that, The mass ratio of the cyclic ketone, the first oxidant, the second solvent, and the catalyst is 1:1-4:10-40:0.05-0.3; And / or, the cyclic ketone is selected from at least one of cyclopentanone, 2-methylcyclohexanone, cyclohexanone, 4-methylcyclohexanone, and 4-ethylcyclohexanone; And / or, the first oxidant is selected from at least one of benzaldehyde, p-methylbenzaldehyde, isobutyraldehyde, and n-butyraldehyde; And / or, the second solvent is selected from at least one of acetonitrile, ethyl acetate and 1,2-dichloroethane.
13. The method according to claim 12, characterized in that, The mass ratio of the cyclic ketone, the first oxidant, the second solvent, and the catalyst is 1:1.5-3:15-30:0.08-0.
2.
14. The method according to any one of claims 1-5, characterized in that, The second oxidant is selected from an oxygen-containing gas, and the concentration of oxygen in the second oxidant is 10-30% by volume. And / or, the second oxidant is air; And / or, the flow rate of the second oxidant is 10-40 mL / min; And / or, the temperature of the catalytic reaction is 30-60°C; And / or, the catalytic reaction takes 6-12 hours.
15. The method according to claim 14, wherein, The flow rate of the second oxidant is 20-40 mL / min; And / or, the catalytic reaction temperature is 40-50°C; And / or, the catalytic reaction time is 8-10 h.
Citation Information
Patent Citations
Method for preparing organic lactone
CN102702152A
Method for preparing organic lactone
CN102603447A