Pn junction semiconductor catalyst for synergistically controlling ozone and nitrogen oxides, and preparation method and application thereof
Patent Information
- Application Number
- CN202211379893.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-04
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-11-04
AI Technical Summary
[0008]本发明的目的是为了克服现有技术存在的空气或废气中O3和N2O或NO等氮氧化物在常温常压下不能自发协同反应问题,提供一种协同控制臭氧和氮氧化物的PN结半导体催化剂及其制备方法和应用,该PN结半导体催化剂具有在常温常压下即可高效促进臭氧与氮氧化物发生反应的显著优势
Abstract
Description
Technical Field
[0001] This invention relates to the field of ambient air and exhaust gas treatment technology, specifically to a PN junction semiconductor catalyst for synergistic control of ozone and nitrogen oxides, its preparation method, and its application. Background Technology
[0002] The top ten greenhouse gases are H2O, CO2, CH4, N2O, O3, CHF3, fluoroethane, sulfur hexafluoride, trichlorofluoromethane, and sulfuryl fluoride.
[0003] Nitrous oxide, ranked fourth among greenhouse gases, is a potent greenhouse gas, and scientists have recently proposed that it plays a catalytic role in the destruction of the atmospheric ozone layer. Forest fires were previously considered the primary source of nitrous oxide. However, in reality, they only account for 7% of the nitrous oxide in the atmosphere. Chemists point out that 10% of nitrous oxide is produced during nylon production. Scientists estimate that the atmospheric concentration of nitrous oxide increases by about 1% every five years, and if left uncontrolled, this will exacerbate the greenhouse effect. The decomposition of N2O generally employs thermal decomposition and thermocatalytic decomposition. Thermal decomposition requires a temperature of 850℃, and catalysts typically include hydrotalcite and spinel-like catalysts (CuAl2O4) or ZrO2 catalysts supported on CoO and NiO, with a catalytic window temperature above 300℃ (from Zhang Yuanyang's doctoral dissertation at East China University of Science and Technology, "Catalytic Decomposition of Greenhouse Gas N2O—Preparation and Performance Study of Composite Metal Oxide Catalysts"). It is evident that both thermal decomposition and thermocatalytic decomposition reactions of N2O are difficult to occur at room temperature.
[0004] Ozone (O3), ranked fifth, has a dual role in the atmosphere: one is a protector of the Earth, the other a pollutant. In the stratosphere, ozone protects the Earth, but in the troposphere, O3 is a pollutant and a significant greenhouse gas. Tropospheric O3 not only absorbs long-wave radiation from the Earth-atmosphere system, thus heating the atmosphere, but also participates in atmospheric photochemical reactions, thereby altering the content and distribution of other greenhouse gases and affecting the radiation balance of the Earth-atmosphere system. In particular, high concentrations of near-surface O3 (from the ground to about 2 km) can trigger urban photochemical smog, affecting human health and severely impacting vegetation and crops. Therefore, tropospheric O3 is called "bad ozone," and its concentration needs to be reduced.
[0005] Therefore, how to reduce ozone and nitrogen oxides such as N2O in the atmosphere, and how to promote the spontaneous reaction of O3 and nitrogen oxides such as N2O or NO in the air or exhaust gas at normal temperature and pressure have become urgent problems to be solved.
[0006] Patent application CN111939888A provides a method for preparing a support material, the support material, a NO oxidation catalyst and its application, but the NO oxidation catalyst can only oxidize NO alone and does not construct a PN junction structure.
[0007] US Patent 7438878B2 discloses a method for the selective catalytic reduction of N2O, which can react N2O and NO. x It is reduced to N2, but in this method, the selective catalytic reduction of N2O still needs to be carried out at a relatively high temperature. Summary of the Invention
[0008] The purpose of this invention is to overcome the problem that nitrogen oxides such as O3 and N2O or NO in air or exhaust gas cannot spontaneously and synergistically react under normal temperature and pressure in the existing technology, and to provide a PN junction semiconductor catalyst for synergistic control of ozone and nitrogen oxides, its preparation method and application. This PN junction semiconductor catalyst has the significant advantage of efficiently promoting the reaction of ozone and nitrogen oxides under normal temperature and pressure.
[0009] To achieve the above objectives, the present invention provides a PN junction semiconductor catalyst for synergistic control of ozone and nitrogen oxides, wherein the PN junction semiconductor catalyst contains a P-type semiconductor material and an N-type semiconductor material;
[0010] The P-type semiconductor material is selected from one or more of SiN, SiP, InSb, HgTe, CdTe and SiC;
[0011] The N-type semiconductor material is MnO doped with the transition metal element M. x We obtain the value where x is between 1 and 3.
[0012] Preferably, the molar ratio of the N-type semiconductor material to the P-type semiconductor material is 1:0.01-1.
[0013] Preferably, the transition metal element M is selected from one or more of Ni, Fe, Co, Ti and W.
[0014] Preferably, the PN junction semiconductor catalyst further contains a matrix material.
[0015] More preferably, the matrix material is selected from catalyst supports and / or catalyst substrates.
[0016] Preferably, the catalyst support is selected from one or more of molecular sieves, zeolites, activated carbon, Al2O3 and ZrO2.
[0017] Preferably, the pore diameter of the catalyst support is 0.3-0.35 nm.
[0018] Preferably, the length of the catalyst support is 3-10 mm.
[0019] Preferably, the catalyst support is rod-shaped, granular, or fibrous.
[0020] Preferably, the catalyst substrate is selected from one or more of glass, conductive coatings, and metals.
[0021] A second aspect of the present invention provides a method for preparing the above-mentioned PN junction semiconductor catalyst, the method comprising the following steps:
[0022] MnO x The N-type semiconductor material is obtained by calcining a mixture of the N-type semiconductor material with an oxide and / or carbonate of a transition metal element M; the N-type semiconductor material, the P-type semiconductor material, and an optional substrate material are then combined.
[0023] Preferably, the molar ratio of Mn to Ni is 1:0-0.2.
[0024] More preferably, the molar ratio of Mn to Fe is 1:0-0.2.
[0025] More preferably, the molar ratio of Mn to Co is 1:0-0.2.
[0026] More preferably, the molar ratio of Mn to Ti is 1:0-0.7.
[0027] More preferably, the molar ratio of Mn to W is 1:0-0.7.
[0028] Preferably, the calcination conditions include: a temperature of 100-500℃, a time of 1-600 min, and an atmosphere of air and / or ammonia.
[0029] Preferably, when the roasting atmosphere is a mixture of air and ammonia, the volume ratio of ammonia to air is 0.05-0.2:100.
[0030] Preferably, the molar ratio of the N-type semiconductor material to the P-type semiconductor material is 1:0.01-1.
[0031] A third aspect of the present invention provides the application of the above-described PN junction semiconductor catalyst in reducing the concentration of ozone and nitrogen oxides in the air.
[0032] The PN junction semiconductor catalyst obtained by this invention has the significant advantage of efficiently promoting the reaction of ozone and nitrogen oxides at room temperature and pressure. Detailed Implementation
[0033] The following provides a detailed description of specific embodiments of the present invention. It should be understood that the specific embodiments described herein are for illustrative and explanatory purposes only and are not intended to limit the scope of the invention.
[0034] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0035] In one aspect, the present invention provides a PN junction semiconductor catalyst for synergistic control of ozone and nitrogen oxides, wherein the PN junction semiconductor catalyst contains a P-type semiconductor material and an N-type semiconductor material;
[0036] The P-type semiconductor material is selected from one or more of SiN, SiP, InSb, HgTe, CdTe and SiC;
[0037] The N-type semiconductor material is MnO doped with the transition metal element M. x We obtain the value where x is between 1 and 3.
[0038] In the PN junction semiconductor catalyst of the present invention, the molar ratio of the N-type semiconductor material to the P-type semiconductor material can be 1:0.01-1.
[0039] In a preferred embodiment of the present invention, the molar ratio of the N-type semiconductor material to the P-type semiconductor material is preferably 1:0.5-1.
[0040] In a specific embodiment of the present invention, the molar ratio of the N-type semiconductor material to the P-type semiconductor material can be 1:0.5, 1:0.55, 1:0.6, 1:0.65, 1:0.7, 1:0.75, 1:0.8, 1:0.85, 1:0.9, 1:0.95 or 1:1.
[0041] In the PN junction semiconductor catalyst of the present invention, the transition metal element M may be selected from one or more of Ni, Fe, Co, Ti and W.
[0042] In this invention, the PN junction semiconductor catalyst may also contain a matrix material.
[0043] In this invention, when the PN junction semiconductor catalyst also contains a matrix material, the P-type semiconductor material and the N-type semiconductor material are loaded on the matrix material.
[0044] In the PN junction semiconductor catalyst of the present invention, in a preferred embodiment, the ratio of the total weight of the P-type semiconductor material and the N-type semiconductor material to the weight of the matrix material is 0.001-0.1:1.
[0045] In the PN junction semiconductor catalyst of the present invention, in a specific embodiment, the ratio of the total weight of the P-type semiconductor material and the N-type semiconductor material to the weight of the matrix material can be 0.001:1, 0.005:1, 0.01:1, 0.015:1, 0.02:1, 0.025:1, 0.03:1, 0.035:1, 0.04:1, 0.045:1, 0.05:1, 0.055:1, 0.06:1, 0.065:1, 0.07:1, 0.075:1, 0.08:1, 0.085:1, 0.09:1, 0.095:1, or 0.1:1.
[0046] In the PN junction semiconductor catalyst of the present invention, in a preferred embodiment, the matrix material is selected from catalyst support and / or catalyst substrate.
[0047] In the PN junction semiconductor catalyst described in this invention, the catalyst support can be a catalyst support commonly used in the art.
[0048] In the PN junction semiconductor catalyst of the present invention, in a preferred embodiment, the catalyst support is selected from one or more of molecular sieves, zeolites, activated carbon, Al2O3 and ZrO2.
[0049] In the PN junction semiconductor catalyst of the present invention, in a preferred embodiment, the pore diameter of the catalyst support is 0.3-0.35 nm.
[0050] In the PN junction semiconductor catalyst of the present invention, in a preferred embodiment, the length of the catalyst support is 3-10 mm.
[0051] In the PN junction semiconductor catalyst of the present invention, in a specific embodiment, the catalyst support can be rod-shaped, granular, or fibrous.
[0052] In the PN junction semiconductor catalyst of the present invention, in a preferred embodiment, the catalyst substrate is selected from one or more of glass, conductive coating and metal.
[0053] A second aspect of the present invention provides a method for preparing the above-mentioned PN junction semiconductor catalyst, the method comprising the following steps:
[0054] MnO xThe N-type semiconductor material is obtained by calcining a mixture of the N-type semiconductor material with an oxide and / or carbonate of a transition metal element M; the N-type semiconductor material, the P-type semiconductor material, and an optional substrate material are then combined.
[0055] In the method for preparing a PN junction semiconductor catalyst described in this invention, in a specific embodiment, MnO can be used. x After mixing with oxides and / or carbonates of transition metal element M, the mixture is calcined to obtain an N-type semiconductor material. Then, the N-type semiconductor material, the P-type semiconductor material, and an optional substrate material are combined.
[0056] In the method for preparing a PN junction semiconductor catalyst described in this invention, in a specific embodiment, MnO can also be used. x MnO is mixed with oxides and / or carbonates of transition metal element M, p-type semiconductor materials, and optional matrix materials before calcination. x (N-type semiconductor material is obtained by calcining oxides and / or carbonates of transition metal element M).
[0057] In one specific embodiment of the method for preparing a PN junction semiconductor catalyst according to the present invention, MnO is used. x After mixing with oxides and / or carbonates of transition metal element M, N-type semiconductor material is obtained by calcination. Then, N-type semiconductor material and P-type semiconductor material are loaded onto a substrate material. The loading method can be chemical vapor deposition, plasma grafting, spraying, brushing, coating, impregnation or extrusion molding.
[0058] In the method for preparing a PN junction semiconductor catalyst according to the present invention, the MnO x It can be selected from one or more of MnO, MnO2 and Mn3O4, or it can also be selected from Mn ore.
[0059] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a preferred embodiment, the MnO x It is MnO2 or Mn ore.
[0060] In the method for preparing a PN junction semiconductor catalyst according to the present invention, the transition metal element M may be selected from one or more of Ni, Fe, Co, Ti and W.
[0061] In the method for preparing a PN junction semiconductor catalyst described in this invention, the molar ratio of Mn to Ni is 1:0-0.2.
[0062] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a preferred embodiment, the molar ratio of Mn element to Ni element is 1:0-0.1.
[0063] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a more preferred case, the molar ratio of Mn element to Ni element is 1:0-0.05.
[0064] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a specific embodiment, the molar ratio of Mn element to Ni element can be 1:0, 1:0.01, 1:0.015, 1:0.02, 1:0.025, 1:0.03, 1:0.035, 1:0.04, 1:0.045 or 1:0.05.
[0065] In the method for preparing a PN junction semiconductor catalyst described in this invention, the molar ratio of Mn to Fe is 1:0-0.2.
[0066] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a preferred embodiment, the molar ratio of Mn to Fe is 1:0-0.1.
[0067] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a more preferred case, the molar ratio of Mn element to Fe element is 1:0-0.03.
[0068] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a specific embodiment, the molar ratio of Mn element to Fe element can be 1:0, 1:0.01, 1:0.015, 1:0.02, 1:0.025, or 1:0.03.
[0069] In the method for preparing a PN junction semiconductor catalyst described in this invention, the molar ratio of Mn to Co is 1:0-0.2.
[0070] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a preferred embodiment, the molar ratio of Mn to Co is 1:0-0.1.
[0071] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a more preferred case, the molar ratio of Mn element to Co element is 1:0-0.05.
[0072] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in specific embodiments, the molar ratio of Mn element to Co element can be 1:0, 1:0.01, 1:0.015, 1:0.02, 1:0.025, 1:0.03, 1:0.035, 1:0.04, 1:0.045 or 1:0.05.
[0073] In the method for preparing a PN junction semiconductor catalyst described in this invention, the molar ratio of Mn to Ti is 1:0-0.7.
[0074] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a preferred embodiment, the molar ratio of Mn to Ti is 1:0-0.5.
[0075] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a specific embodiment, the molar ratio of Mn element to Ti element can be 1:0, 1:0.1, 1:0.15, 1:0.2, 1:0.25, 1:0.3, 1:0.35, 1:0.4, 1:0.45 or 1:0.5.
[0076] In the method for preparing a PN junction semiconductor catalyst described in this invention, the molar ratio of Mn to W is 1:0-0.7.
[0077] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a preferred embodiment, the molar ratio of Mn to W is 1:0-0.5.
[0078] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a specific embodiment, the molar ratio of Mn element to W element can be 1:0, 1:0.1, 1:0.15, 1:0.2, 1:0.25, 1:0.3, 1:0.35, 1:0.4, 1:0.45 or 1:0.5.
[0079] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a preferred embodiment, in order to obtain a N-type semiconductor material with better performance, the calcination conditions include: a temperature of 100-500°C, a time of 1-600 min, and an atmosphere of air and / or ammonia.
[0080] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a preferred embodiment, the calcination temperature is 300-500°C and the calcination time is 60-300 min.
[0081] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a specific embodiment, the calcination temperature can be 300℃, 310℃, 320℃, 330℃, 340℃, 350℃, 360℃, 370℃, 380℃, 390℃, 400℃, 410℃, 420℃, 430℃, 440℃, 450℃, 460℃, 470℃, 480℃, 490℃, or 500℃.
[0082] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a specific embodiment, the calcination time can be 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min, 180 min, 190 min, 200 min, 210 min, 220 min, 230 min, 240 min, 250 min, 260 min, 270 min, 280 min, 290 min, or 300 min.
[0083] In the method for preparing a PN junction semiconductor catalyst according to the present invention, when the calcination atmosphere is a mixture of air and ammonia, the volume ratio of ammonia to air is 0.05-0.2:100.
[0084] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a specific embodiment, the volume ratio of ammonia to air can be 0.05:100, 0.06:100, 0.07:100, 0.08:100, 0.09:100, 0.1:100, 0.11:100, 0.12:100, 0.13:100, 0.14:100, 0.15:100, 0.16:100, 0.17:100, 0.18:100, 0.19:100, or 0.2:100.
[0085] In the method for preparing a PN junction semiconductor catalyst according to the present invention, the molar ratio of the N-type semiconductor material to the P-type semiconductor material is 1:0.01-1.
[0086] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a preferred embodiment, the molar ratio of the N-type semiconductor material to the P-type semiconductor material is 1:0.5-1.
[0087] In the method for preparing a PN junction semiconductor catalyst according to the present invention, in a specific embodiment, the molar ratio of the N-type semiconductor material to the P-type semiconductor material can be 1:0.5, 1:0.55, 1:0.6, 1:0.65, 1:0.7, 1:0.75, 1:0.8, 1:0.85, 1:0.9, 1:0.95, or 1:1.
[0088] A third aspect of the present invention provides the application of the above-described PN junction semiconductor catalyst in reducing the concentration of ozone and nitrogen oxides in the air.
[0089] The PN junction semiconductor catalyst described in this invention can be mixed into the topcoat of water-based wall paints and waterproof coatings; sprayed into the waterproof coating of building roofs; or sprayed, brushed, or impregnated onto the glass surface by methods such as chemical vapor deposition, plasma grafting, or dissolving in glass adhesives; or used in air purifier filters, ozone catalytic oxidation exhaust gas decomposers, and plasma waste gas treatment exhaust gas decomposers to reduce the content of ozone and nitrogen oxides in the air.
[0090] When the PN junction semiconductor catalyst described in this invention is used in the topcoat of water-based wall paint, 0.01 to 0.5 wt% of the PN junction semiconductor catalyst is added to 1 L of the topcoat of water-based wall paint.
[0091] In a specific embodiment, the addition ratio of the PN junction semiconductor catalyst in the topcoat of 1L of water-based wall paint can be 0.01wt%, 0.05wt%, 0.1wt%, 0.15wt%, 0.2wt%, 0.25wt%, 0.3wt%, 0.35wt%, 0.4wt%, 0.45wt%, or 0.5wt%.
[0092] When the PN junction semiconductor catalyst described in this invention is sprayed onto a building roof waterproof coating, before the waterproof coating dries, within 1m... 2 A 1μm thick PN junction semiconductor catalyst thin layer is sprayed onto the roof synthetic polymer waterproof membrane or polymer modified bitumen waterproof membrane using an adhesive as a solvent.
[0093] When the PN junction semiconductor catalyst described in this invention is used in a waterproof coating, the PN junction semiconductor catalyst is directly mixed in a ratio of 0.01 to 0.5 wt% into a synthetic polymer waterproof coating, a single-component water-curing polyurethane waterproof coating, or a cement-based penetrating crystalline waterproof coating.
[0094] In a specific embodiment, when the PN junction semiconductor catalyst is mixed in the waterproof coating, the mixing ratio of the PN junction semiconductor catalyst can be 0.01wt%, 0.05wt%, 0.1wt%, 0.15wt%, 0.2wt%, 0.25wt%, 0.3wt%, 0.35wt%, 0.4wt%, 0.45wt%, or 0.5wt%.
[0095] When the PN junction semiconductor catalyst described in this invention is used in air purifier filters, ozone catalytic oxidation exhaust gas decomposers, and plasma waste gas treatment exhaust gas decomposers, at a space velocity of 4000-40000 h⁻¹, -1 The proportion of filling can be 4000h. -1 5000h -1 7000h -1 10000h-1 12000h -1 15000h -1 17000h -1 20000h -1 23000h -1 25000h -1 27000h -1 30000h -1 33000h -1 35000h -1 37000h -1 or 40000h -1 .
[0096] In this invention, "airspeed" refers to "volume airspeed".
[0097] In the atmosphere, nitrous oxide does not react with O2, but slowly generates NO under ultraviolet light. NO then reacts with strong oxidizing agents such as O3 to produce NO2 and NO3. - When ozone encounters H₂, OH₂, NO, Cl₂, Br₂, or an ozone decomposition catalyst, such as on the catalyst surface, ozone gains electrons and is catalytically decomposed into O₂ and active M₂. (n+1) + —O - At this point, the active oxygen atoms possess high oxidizing power, rapidly oxidizing N₂O and NO to NO and NO₂, while simultaneously consuming ozone. The controlling step of the reaction is the adsorption process of N₂O and O₃ on the catalyst surface. Ozone is nucleophilic, and the catalyst surface exposes more positive charges, which greatly promotes the adsorption of ozone on the active sites of the catalyst, promoting the ozone decomposition reaction, and thus promoting the oxidation reaction of N₂O and NO.
[0098] To enable O3 to spontaneously react with N2O or NO at room temperature and pressure, more oxygen vacancies or positive charges need to be exposed on the catalyst surface to promote O3 adsorption. The adsorbed O3 generates active oxygen under the action of the catalyst. At the same time, materials and special structures that easily adsorb N2O or NO are constructed on the surface near the active sites of the ozone decomposition catalyst, so that more negative charges are also exposed on the catalyst surface to promote the adsorption of N2O or NO, thereby promoting the reaction of N2O or NO with the active oxygen decomposition products of O3.
[0099] Furthermore, to expose positive charges in some areas and negative charges in others on the catalyst surface, this can be achieved by constructing materials with semiconductor structures. Semiconductors are materials whose conductivity at room temperature falls between that of conductors and insulators. Common semiconductor materials include silicon, germanium, and gallium arsenide. Semiconductors also exist in various forms, including solids, liquids, and plasmas. Under the influence of light or electricity, semiconductor materials generate photo- or electro-charges, causing electrons in the baseband to jump to the conduction band, resulting in a positive charge in the baseband, which becomes the valence band, facilitating ozone adsorption. However, electrons that jump to the conduction band easily return to the valence band and recombine with holes. However, utilizing the principle of PN junctions, by doping or depositing P-type semiconductor materials such as SiN, SiP, InSb, HgTe, CdTe, and SiC (which readily adsorb N₂O or NO) into N-type semiconductor materials, a PN junction can be constructed, which facilitates the migration of electrons from the N-type semiconductor and holes from the P-type semiconductor to the PN junction interface.
[0100] In order to promote the adsorption of N2O or NO in P semiconductor materials such as SiN, SiP, InSb, HgTe, CdTe and SiC, confined pore structures suitable for the dissolution and diffusion of N2O and NO can be constructed.
[0101] To promote the participation of more O3 and N2O or NO in the reaction, catalytic materials with a PN junction structure can be sprayed onto the surface of the roof waterproof felt, the exterior walls of buildings, and the interior wall materials.
[0102] Compared with traditional N2O treatment technologies, the PN junction semiconductor catalyst of this invention has the characteristics of selective adsorption of O3 by N-type semiconductors and selective adsorption of N2O or NO by P-type semiconductors, and the reaction efficiency of N2O or NO with active oxygen atoms on the PN junction surface is significantly improved (this is because after the N-type semiconductor decomposes O3, M... (n+1) + —O - Electrons on oxygen atoms migrate more easily towards p-type semiconductors, which can significantly improve the decomposition effect of O3 and the adsorption effect of N2O or NO on p-type semiconductors. Relying on the active oxygen generated during the catalytic decomposition of O3 at room temperature, it can undergo an oxidation reaction with N2O or NO at room temperature and pressure. It has the significant advantage of being able to efficiently react ozone with N2O or NO at room temperature and pressure. By utilizing O3 in the air, N2O is oxidized into NO and NO2, while consuming ozone and reducing the content of ozone and nitrogen oxides in the air.
[0103] Compared with traditional PN junction substrates, the pores of the PN junction semiconductor catalyst described in this invention are conducive to the dissolution and diffusion of N2O / NO, but not conducive to the dissolution and diffusion of H2O / N2 / O2.
[0104] Compared with traditional ozone decomposition catalysts or N2O catalytic oxidation catalysts, the PN junction semiconductor catalyst of this invention has photosensitivity and can significantly enhance the synergistic control of ozone and nitrogen oxides in the air under external visible / ultraviolet light irradiation.
[0105] The PN junction semiconductor catalyst described in this invention has the function of long-term treatment of O3 and N2O in the atmosphere, and the effect is even better under light.
[0106] The present invention will be described in detail below through embodiments, but the methods described in the present invention are not limited thereto.
[0107] The Mn ore used in the following examples are all commercially available products.
[0108] Example 1
[0109] (1) MnO2 and CoCO3 were mixed in a molar ratio of 1:0.05 and then calcined in air at 350°C for 2 hours to obtain N-type semiconductor material.
[0110] (2) The obtained N-type semiconductor material and SiN powder (P-type semiconductor material) are mixed at a molar ratio of 1:1 to obtain a mixture. The mixture is then mixed with ethanol at a weight ratio of 0.001:1. After being ultrasonically dispersed evenly, the mixture is impregnated onto activated carbon fiber material with a pore diameter of 0.3-0.35 nm and a length of 3-10 mm (the weight ratio of the mixture to the activated carbon fiber material is 0.05:1). After drying at 80°C, a PN junction semiconductor catalyst is obtained for later use.
[0111] The PN junction semiconductor catalyst prepared in this example was packed into the middle section of a glass tube, and air containing 100 ppm O3 and 110 ppm N2O was introduced at a space velocity of 4000 h⁻¹. -1 At room temperature (20°C) and atmospheric pressure, the O3 content in the gas at the outlet was measured to be 1.0 ppm and the N2O content to be 2.5 ppm.
[0112] Example 2
[0113] (1) MnO2 and titanium dioxide are mixed in a ratio of 1:0.1, and then calcined in air at 350°C for 2 hours to obtain N-type semiconductor material.
[0114] (2) The obtained N-type semiconductor material and silicon phosphide powder (P-type semiconductor material) are mixed at a molar ratio of 1:0.5 to obtain a mixture. The mixture is then mixed with ethanol at a weight ratio of 0.001:1. After being ultrasonically dispersed evenly, the mixture is impregnated onto ZSM-5 molecular sieve rods with a pore diameter of 0.3-0.35 nm and a length of 3-10 mm (the weight ratio of the mixture to the ZSM-5 molecular sieve rods is 0.05:1). After drying at 80 °C, a PN junction semiconductor catalyst is obtained for later use.
[0115] The PN junction semiconductor catalyst prepared in this embodiment was packed into the middle section of a glass tube, and air containing 100 ppm O3 and 110 ppm N2O was introduced at a space velocity of 4000 h⁻¹. -1 At room temperature of 20°C and atmospheric pressure, the O3 content in the gas at the outlet was measured to be 2.5 ppm and the N2O content to be 8.9 ppm.
[0116] Example 3
[0117] (1) MnO2 and Fe3O4 were mixed in a molar ratio of 1:0.01 and then calcined in air at 500°C for 5 hours to obtain N-type semiconductor material.
[0118] (2) The obtained N-type semiconductor material and CdTe (P-type semiconductor material) are mixed in a molar ratio of 1:1 to obtain a mixture. The mixture is then mixed with ethanol in a weight ratio of 0.001:1. After being ultrasonically dispersed evenly, the mixture is impregnated onto activated carbon fiber material with a pore diameter of 0.3-0.35 nm and a length of 3-10 mm (the weight ratio of the mixture to the activated carbon fiber material is 0.05:1). After drying at 80 °C, a PN junction semiconductor catalyst is obtained for later use.
[0119] The PN junction semiconductor catalyst prepared in this embodiment was packed into the middle section of a glass tube, and air containing 100 ppm O3 and 110 ppm N2O was introduced at a space velocity of 4000 h⁻¹. -1 At room temperature (20°C) and atmospheric pressure, the O3 content in the gas at the outlet was measured to be 6.5 ppm and the N2O content to be 5.0 ppm.
[0120] Example 4
[0121] (1) Mn ore and tungsten ore are mixed in a ratio of 1:0.45 for the amount of Mn in the Mn ore to W in the tungsten ore, and then roasted at 450°C for 4 hours. The roasting atmosphere is a mixture of air and ammonia, with a volume ratio of ammonia to air of 0.15:100, to obtain N-type semiconductor material.
[0122] (2) The obtained N-type semiconductor material and SiC powder (P-type semiconductor material) are mixed at a molar ratio of 1:0.7 to obtain a mixture. The mixture is then mixed with ethanol at a weight ratio of 0.001:1. After being ultrasonically dispersed evenly, the mixture is impregnated onto activated carbon fiber material with a pore diameter of 0.3-0.35 nm and a length of 3-10 mm (the weight ratio of the mixture to the activated carbon fiber material is 0.05:1). After drying at 80°C, a PN junction semiconductor catalyst is obtained for later use.
[0123] The PN junction semiconductor catalyst prepared in this embodiment was packed into the middle section of a glass tube, and air containing 100 ppm O3 and 110 ppm N2O was introduced at a space velocity of 4000 h⁻¹. -1 At room temperature (20°C) and atmospheric pressure, the O3 content in the gas at the outlet was measured to be 7.5 ppm and the N2O content to be 6.5 ppm.
[0124] Example 5
[0125] (1) Mn ore and titanium dioxide are mixed in a ratio of 1:0.3 for the amount of Mn element in Mn ore to Ti element in titanium dioxide. The mixture is then calcined at 400°C for 5 hours in an atmosphere of air and ammonia with a volume ratio of 100:0.15 to obtain N-type semiconductor material.
[0126] (2) The obtained N-type semiconductor material and SiC powder (P-type semiconductor material) are mixed at a molar ratio of 1:0.9 to obtain a mixture. The mixture is then mixed with ethanol at a weight ratio of 0.001:1. After being ultrasonically dispersed evenly, the mixture is impregnated onto activated carbon fiber material with a pore diameter of 0.3-0.35 nm and a length of 3-10 mm (the weight ratio of the mixture to the activated carbon fiber material is 0.06:1). After drying at 80 °C, a PN junction semiconductor catalyst is obtained for later use.
[0127] The PN junction semiconductor catalyst prepared in this embodiment was packed into the middle section of a glass tube, and air containing 100 ppm O3 and 110 ppm N2O was introduced at a space velocity of 4000 h⁻¹. -1 At room temperature (20°C) and atmospheric pressure, the O3 content in the gas at the outlet was measured to be 5.5 ppm and the N2O content to be 8.0 ppm.
[0128] Example 6
[0129] (1) MnO2 and Fe3O4 were mixed in a molar ratio of 1:0.008 and then calcined at 300°C for 4 hours. The calcination atmosphere was air and ammonia, and the volume ratio of air to ammonia was 100:0.2 to obtain N-type semiconductor material.
[0130] (2) The obtained N-type semiconductor material and CdTe (P-type semiconductor material) are mixed at a molar ratio of 1:0.8 to obtain a mixture. The mixture is then mixed with ethanol at a weight ratio of 0.001:1. After being ultrasonically dispersed evenly, the mixture is impregnated onto activated carbon fiber material with a pore diameter of 0.3-0.35 nm and a length of 3-10 mm (the weight ratio of the mixture to the activated carbon fiber material is 0.07:1). After drying at 80°C, a PN junction semiconductor catalyst is obtained for later use.
[0131] The PN junction semiconductor catalyst prepared in this embodiment was packed into the middle section of a glass tube, and air containing 100 ppm O3 and 110 ppm N2O was introduced at a space velocity of 4000 h⁻¹. -1 At room temperature (20°C) and atmospheric pressure, the O3 content in the gas at the outlet was measured to be 5.0 ppm and the N2O content to be 6.0 ppm.
[0132] Example 7
[0133] (1) Mn ore and CoCO3 are mixed in a ratio of 1:0.04 of Mn element in Mn ore to Co element in CoCO3, and then calcined at 450°C for 2.5 h. The calcination atmosphere is air and ammonia, and the volume ratio of air and ammonia is 100:0.2 to obtain N-type semiconductor material.
[0134] (2) The obtained N-type semiconductor material and SiN powder (P-type semiconductor material) are mixed at a molar ratio of 1:0.9 to obtain a mixture. The mixture is then mixed with ethanol at a weight ratio of 0.001:1. After being ultrasonically dispersed evenly, the mixture is impregnated onto activated carbon fiber material with a pore diameter of 0.3-0.35 nm and a length of 3-10 mm (the weight ratio of the mixture to the activated carbon fiber material is 0.07:1). After drying at 80°C, a PN junction semiconductor catalyst is obtained for later use.
[0135] The PN junction semiconductor catalyst prepared in this example was packed into the middle section of a glass tube, and air containing 100 ppm O3 and 110 ppm N2O was introduced at a space velocity of 4000 h⁻¹. -1 At room temperature (20°C) and atmospheric pressure, the O3 content in the gas at the outlet was measured to be 3.0 ppm and the N2O content to be 2.0 ppm.
[0136] Example 8
[0137] MnO2 and WO3 were mixed in a molar ratio of 1:0.1, and then mixed with InSb (P-type semiconductor material) to obtain a mixture. The mixture was then mixed with ethanol at a weight ratio of 0.001:1, and Al2O3 powder with a pore diameter of 0.3-0.35 nm was added. After ultrasonic dispersion, the mixture was extruded into rods with a length of 3-10 mm, and then calcined in air at 400℃ for 5 h (after calcination, MnO2 and WO3 were used to obtain N-type semiconductor material) to obtain a PN junction semiconductor catalyst for later use (the molar ratio of N-type semiconductor material to P-type semiconductor material was 1:1, and the total weight of N-type semiconductor material and P-type semiconductor material was 0.05:1 compared with the weight of Al2O3 powder material).
[0138] The PN junction semiconductor catalyst prepared in this embodiment was packed into the middle section of a glass tube, and air containing 100 ppm O3 and 110 ppm N2O was introduced at a space velocity of 4000 h⁻¹. -1 At room temperature of 20°C and atmospheric pressure, the O3 content in the gas at the outlet was measured to be 2.1 ppm and the N2O content to be 13.2 ppm.
[0139] Comparative Example 1
[0140] The purchased hydrotalcite and spinel-like catalyst (CuAl2O4) from BASF were used. The hydrotalcite and spinel-like catalyst (CuAl2O4) were packed into the middle section of a glass tube, and air containing 100 ppm O3 and 110 ppm N2O was introduced at a space velocity of 4000 h⁻¹. -1 The inlet temperature was 320℃, the pressure was atmospheric pressure, and the O3 content in the outlet gas was measured to be 20.3ppm and the N2O content was 15.5ppm.
[0141] Example 9
[0142] (1) Mn ore and NiO are mixed in a ratio of 1:0.05 between the amount of Mn in Mn ore and the amount of Ni in NiO, and then calcined in air at 300°C for 2 hours to obtain N-type semiconductor material.
[0143] (2) Mix N-type semiconductor material with ethanol at a weight ratio of 0.001:1, disperse evenly by ultrasonication, and then spray evenly onto a glass plate coated with a silicon carbide (P-type semiconductor material) film (the molar ratio of N-type semiconductor material to P-type semiconductor material is 1:0.5, and the ratio of the total weight of N-type semiconductor material and P-type semiconductor material to the weight of the glass plate is 0.05:1). After drying at 80°C, a PN junction semiconductor catalyst is obtained for later use.
[0144] Multiple PN junction semiconductor catalyst sheets prepared in this embodiment were packed side-by-side (0.5 mm apart) in the middle section of a square glass tube. Air containing 100 ppm O3 and 110 ppm N2O was introduced, with the amount of gas introduced being equal to the internal volume of the square glass tube. At room temperature (20°C) and atmospheric pressure, the O3 content inside the square glass tube was measured to be 5.0 ppm and the N2O content to be 14 ppm after 10 hours.
[0145] Example 10
[0146] (1) Mn ore and titanium dioxide are mixed in a ratio of 1:0.5 of Mn element in Mn ore to Ti element in titanium dioxide, and then calcined in air at 350°C for 2 hours to obtain N-type semiconductor material.
[0147] (2) The obtained N-type semiconductor material and SiC powder (P-type semiconductor material) are mixed in a molar ratio of 1:1 to obtain a mixture. The mixture is then mixed with ethanol in a weight ratio of 0.001:1. After being ultrasonically dispersed evenly, the mixture is evenly sprayed onto a glass slide (the weight ratio of the mixture to the glass slide is 0.05:1). After drying at 80°C, a PN junction semiconductor catalyst is obtained for later use.
[0148] Multiple PN junction semiconductor catalyst sheets were packed side-by-side (0.5 mm apart) in the middle section of a square glass tube. High-pressure mercury lamps were irradiated at both ends of the square glass tube, and air containing 100 ppm O3 and 110 ppm N2O was introduced. The amount of gas introduced was equal to the internal volume of the square glass tube. At room temperature (20°C) and atmospheric pressure, the O3 content inside the square glass tube was measured to be 1.5 ppm and the N2O content to be 2.5 ppm after 10 hours.
[0149] Example 11
[0150] (1) Mn ore and titanium dioxide are mixed in a ratio of 1:0.5 of Mn element in Mn ore to Ti element in titanium dioxide, and then calcined in air at 350°C for 2 hours to obtain N-type semiconductor material.
[0151] (2) The obtained N-type semiconductor material is mixed with ethanol at a weight ratio of 0.001:1, and after being ultrasonically dispersed evenly, it is uniformly sprayed onto a glass plate coated with a silicon carbide (P-type semiconductor material) film (the molar ratio of N-type semiconductor material to P-type semiconductor material is 1:0.5, and the ratio of the total weight of N-type semiconductor material and P-type semiconductor material to the weight of the glass plate is 0.05:1). After drying at 80°C, a PN junction semiconductor catalyst is obtained for later use.
[0152] Multiple PN junction semiconductor catalyst sheets prepared in this embodiment were packed side-by-side (0.5 mm apart) in the middle section of a square glass tube. The two ends of the square glass tube were not illuminated by high-pressure mercury lamps. Air containing 100 ppm O3 and 110 ppm N2O was introduced, and the amount of gas introduced was equal to the internal volume of the square glass tube. At room temperature of 20°C and atmospheric pressure, the O3 content inside the square glass tube was measured to be 2.9 ppm and the N2O content to be 9.2 ppm after 10 hours.
[0153] Example 12
[0154] (1) Mn ore and tungsten ore are mixed in a ratio of 1:0.5 of Mn element in Mn ore to W element in tungsten ore, and then roasted at 500°C for 5 hours. The roasting atmosphere is air and ammonia, and the volume ratio of air and ammonia is 100:0.1 to obtain N-type semiconductor material.
[0155] (2) The obtained N-type semiconductor material and SiC powder (P-type semiconductor material) are mixed in a molar ratio of 1:1 to obtain a mixture. The mixture is then mixed with ethanol in a weight ratio of 0.001:1. After being ultrasonically dispersed evenly, the mixture is evenly sprayed onto a glass slide (the weight ratio of the mixture to the glass slide is 0.05:1). After drying at 80°C, a PN junction semiconductor catalyst is obtained for later use.
[0156] Multiple PN junction semiconductor catalyst sheets prepared in this embodiment were packed side-by-side (0.5 mm apart) in the middle section of a square glass tube. Xenon lamps were irradiated at both ends of the square glass tube, and air containing 100 ppm O3 and 110 ppm N2O was introduced. The amount of gas introduced was equal to the internal volume of the square glass tube. At room temperature (20°C) and atmospheric pressure, the O3 content inside the square glass tube was measured to be 1.4 ppm and the N2O content to be 2.9 ppm after 10 hours.
[0157] Example 13
[0158] (1) Mn ore and tungsten ore are mixed in a ratio of 1:0.5 of Mn element in Mn ore to W element in tungsten ore, and then roasted at 500°C for 5 hours. The roasting atmosphere is air and ammonia, and the volume ratio of air and ammonia is 100:0.1 to obtain N-type semiconductor material.
[0159] (2) The obtained N-type semiconductor material and SiC powder (P-type semiconductor material) are mixed in a molar ratio of 1:1 to obtain a mixture. The mixture is then mixed with ethanol in a weight ratio of 0.001:1. After being ultrasonically dispersed evenly, the mixture is evenly sprayed onto a glass slide (the weight ratio of the mixture to the glass slide is 0.05:1). After drying at 80°C, a PN junction semiconductor catalyst is obtained for later use.
[0160] Multiple PN junction semiconductor catalyst sheets prepared in this embodiment were packed side-by-side (0.5 mm apart) in the middle section of a square glass tube. The two ends of the square glass tube were not illuminated by xenon lamps. Air containing 100 ppm O3 and 110 ppm N2O was introduced, and the amount of gas introduced was equal to the internal volume of the square glass tube. At room temperature of 20°C and atmospheric pressure, the O3 content inside the square glass tube was measured to be 5.5 ppm and the N2O content to be 15 ppm after 10 hours.
[0161] Example 14
[0162] (1) Mn ore and titanium dioxide are mixed in a ratio of 1:0.5 of Mn element in Mn ore to Ti element in titanium dioxide and then calcined in air at 350°C for 2 hours to obtain N-type semiconductor material.
[0163] (2) The obtained N-type semiconductor material and SiC powder (P-type semiconductor material) are mixed in a molar ratio of 1:1 to obtain a PN junction semiconductor catalyst. The PN junction semiconductor catalyst and the binder are mixed in a weight ratio of 0.001:1, ultrasonically dispersed, and then sprayed onto the polymer-modified bitumen waterproof membrane in a 1μm thin layer.
[0164] A polymer-modified bitumen waterproof membrane coated with the PN junction semiconductor catalyst prepared in this embodiment was laid on the top of the building. The polymer-modified bitumen waterproof membrane coated with the PN junction semiconductor catalyst was covered with a cubic quartz glass dome. Air containing 100 ppm O3 and 110 ppm N2O was introduced, with the amount of gas introduced being equal to the internal volume of the cubic quartz glass dome. After 4 hours of exposure to sunlight at a room temperature of 20°C and a pressure of normal, the O3 content in the cubic quartz glass dome was measured to be 30 ppm and the N2O content to be 39 ppm.
[0165] The test results of the above catalysts show that, compared with existing catalysts, the PN junction semiconductor catalyst prepared by the method of this invention can efficiently promote the reaction of ozone and nitrogen oxides at room temperature and pressure, and effectively reduce the content of ozone and nitrogen oxides. Furthermore, the PN junction semiconductor catalyst of this invention also has photosensitizing properties, and under external visible / ultraviolet light irradiation, it can enhance the synergistic effect of reducing ozone and nitrogen oxides in the air.
[0166] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A PN junction semiconductor catalyst for synergistically controlling ozone and nitrogen oxides, characterized by, The PN junction semiconductor catalyst contains a P-type semiconductor material, an N-type semiconductor material, and a matrix material; The P-type semiconductor material is selected from one or more of SiN, SiP, InSb, HgTe, CdTe and SiC; The N-type semiconductor material is doped with a transition metal element M x is obtained, wherein x is 1-3, and the transition metal element M is selected from one or more of Ni, Fe, Co, Ti, and W. The ratio of the total weight of the P-type semiconductor material and the N-type semiconductor material to the weight of the substrate material is 0.001-0.1:1; the molar ratio of the N-type semiconductor material to the P-type semiconductor material is 1:0.01-1.
2. The PN junction semiconductor catalyst according to claim 1, wherein The matrix material is selected from catalyst supports and / or catalyst substrates.
3. The PN junction semiconductor catalyst according to claim 2, characterized in that, The catalyst support is selected from one or more of molecular sieves, zeolites, activated carbon, Al2O3, and ZrO2.
4. The PN junction semiconductor catalyst according to claim 2 or 3, characterized in that, The catalyst support has a pore diameter of 0.3-0.35 nm.
5. The PN junction semiconductor catalyst according to claim 2 or 3, characterized in that, The length of the catalyst support is 3-10 mm.
6. The PN junction semiconductor catalyst according to claim 4, characterized in that, The catalyst support is rod-shaped, granular, or fibrous.
7. The PN junction semiconductor catalyst according to claim 2 or 3, characterized in that, The catalyst substrate is selected from one or more of glass, conductive coatings, and metals.
8. A method for preparing the PN junction semiconductor catalyst according to any one of claims 1-7, characterized in that, The method includes the following steps: MnO x is mixed with an oxide and / or carbonate of a transition metal element M and is calcined to obtain an N-type semiconductor material; the N-type semiconductor material, a P-type semiconductor material, and a base material are combined.
9. The method according to claim 8, characterized in that, The molar ratio of Mn to Ni is 1:0.01-0.
2.
10. The method according to claim 8, characterized in that, The molar ratio of Mn to Fe is 1:0.01-0.
2.
11. The method according to claim 8, characterized in that, The molar ratio of Mn to Co is 1:0.01-0.
2.
12. The method according to claim 8, characterized in that, The molar ratio of Mn to Ti is 1:0.1-0.
7.
13. The method according to claim 8, characterized in that, The molar ratio of Mn to W is 1:0.1-0.
7.
14. The method according to claim 8, characterized in that, The calcination conditions include: a temperature of 100-500℃, a time of 1-600 min, and an atmosphere of air and / or ammonia.
15. The method according to claim 14, characterized in that, When the roasting atmosphere is a mixture of air and ammonia, the volume ratio of ammonia to air is 0.05-0.2:
100.
16. The method according to claim 8 or 15, characterized in that, The molar ratio of the N-type semiconductor material to the P-type semiconductor material is 1:0.01-1.
17. The use of the PN junction semiconductor catalyst according to any one of claims 1-7 or the PN junction semiconductor catalyst prepared by the method according to any one of claims 8-16 in reducing the concentration of ozone and nitrogen oxides in the air.
Citation Information
Patent Citations
Method for preparing carrier material, carrier material, NO oxidation catalyst and application of NO oxidation catalyst
CN111939888A
Selective catalytic reduction of N2O
US7438878B2
Industrial organic waste gas catalytic degradation catalyst cooperated with low-temperature plasma, and preparation method and application of catalyst
CN105478136A