Production and preparation of long carbon chain modified high melt strength TPU foaming special material

By preparing TPU foam materials modified with long carbon chains, the chemical cross-linking and physical entanglement of molecular chains were enhanced, solving the problems of low melt strength and difficulty in forming pores in TPU foam materials during the foaming process, and achieving higher melt strength and shrinkage resistance.

CN118005879BActive Publication Date: 2026-11-24HEBEI MINGRUN COMPOSITE MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311707505.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-12
Publication Date
2026-11-24
Estimated Expiration
2043-12-12

AI Technical Summary

Technical Problem

Existing TPU foam materials have poor melt strength during the foaming process, and the cell walls are prone to rupture, making it difficult to form pores. Furthermore, the melting temperature is too high to meet the application requirements.

Method used

A long-chain modified high melt strength TPU foam material was synthesized using pentaerythritol, long-chain acids, diisocyanates, polyether diols, chain extenders, and foam stabilizers as raw materials. This method enhances the chemical crosslinking degree of the molecular chains and improves the physical entanglement and cell wall strength.

Benefits of technology

It improves the melt strength and shrinkage resistance of TPU foam materials, solves the problem of cell wall rupture, enhances the ability to form pores, reduces the gas diffusion rate, and improves the heat resistance and molding difficulty of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

This invention provides a method for producing and preparing a long-chain modified high melt strength TPU foam material. The long-chain modified high melt strength TPU foam material is synthesized from pentaerythritol, long-chain acid, diisocyanate, polyether diol, chain extender, catalyst, and foam stabilizer as raw materials. This invention significantly improves the melt strength of the material by increasing the physical entanglement between TPU molecular chains, allowing sufficient deformation space in the cell walls during cell growth. This results in a long-chain modified high melt strength TPU foam material with high foaming ratio and low molding cost that meets application requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer materials technology, specifically to the production and preparation of a long-carbon-chain modified high melt strength TPU foam material. Background Technology

[0002] Thermoplastic polyurethane (TPU) possesses excellent elasticity and cushioning properties, high strength, strong mechanical properties, and good machinability, leading to its wider application in various fields. However, TPU's heavy weight and high hardness limit its applications. TPU foam materials significantly improve upon these shortcomings. Due to its porous structure, TPU foam materials offer advantages such as light weight, good resilience, and strong compression resistance, providing structural support, cushioning, and energy absorption, thus finding a very wide range of applications.

[0003] Currently, the shortcomings of TPU foam materials lie in the lack of chemical cross-linking between molecular chains. This results in poor heat resistance and melt strength. During the foaming process, the cell walls lack sufficient deformation space, making them prone to rupture. Significantly increasing the degree of chemical cross-linking between TPU molecular chains would raise the melting temperature of TPU foam materials, failing to meet practical application requirements. Therefore, research into TPU foam material preparation technology is of great significance in addressing these issues. Developing TPU foam beads with high expansion ratios and low molding costs that meet application requirements will further enhance the market competitiveness of TPU foam materials. Summary of the Invention

[0004] The technical problem to be solved by the present invention is to provide a production and preparation method for a long carbon chain modified high melt strength TPU foaming material, so as to solve the technical problem of poor melt strength of TPU foaming materials in the prior art during the foaming process.

[0005] To solve the above-mentioned technical problems, the technical solution of the present invention is as follows: This high melt strength TPU foaming material with long carbon chain modification is synthesized from pentaerythritol, long carbon chain acid, diisocyanate, polyether diol, chain extender, catalyst and foam stabilizer as raw materials.

[0006] Preferably, the long-chain modified high melt strength TPU foaming material is synthesized from the following raw materials in parts by weight: 100 parts by weight of diisocyanate, 6 parts by weight of pentaerythritol, 12 parts by weight of long-chain acid, 104 parts by weight of polyether diol, 2 parts by weight of chain extender, 3 parts by weight of catalyst, and 2 parts by weight of foam stabilizer.

[0007] Preferably, the long-chain acid is octanoic acid; Preferably, the diisocyanate is p-phenyl diisocyanate; Preferably, the polyether diol is polyether N210; Preferably, the chain extender is 1,4-butanediol; Preferably, the catalyst is dibutyltin dilaurate; Preferably, the foam stabilizer is a copolymer of polyether and silicone oil; Preferably, the diol with a long carbon chain side chain has a structure as shown in formula (I): (I) Where n is an integer greater than or equal to 8.

[0008] This invention also provides a method for preparing the aforementioned long-carbon-chain modified high melt strength TPU foaming material, comprising the following steps: (1) Take pentaerythritol and react it with a long-chain acid to obtain a diol with a long-chain side chain; (2) The diols and diisocyanates with long carbon side chains obtained in step (1) are mixed evenly with polyether diols and reacted to obtain small molecule prepolymers; (3) Add chain extender and foam stabilizer to the small molecule prepolymer obtained in step (2) and react to obtain long carbon chain modified high melt strength TPU material; (4) The long carbon chain modified high melt strength TPU material obtained in step (3) is introduced into a high pressure reactor along with carbon dioxide and foam stabilizer. After adjusting to a suitable temperature, pressure and saturation time, the pressure is quickly released to atmospheric pressure to obtain a long carbon chain modified high melt strength TPU foam material.

[0009] Preferably, in step (1), the reaction temperature is 180-190℃ and the reaction time is 2-3h; Preferably, in step (2), the reaction temperature is 85-120℃ and the reaction time is 3-4h; Preferably, in step (3), the reaction temperature is 140-220℃ and the reaction time is 0.1-1h; Preferably, in step (4), the reaction temperature is 70-80℃ and the reaction time is 4-5h.

[0010] Preferably, step (1) specifically includes: adding pentaerythritol and long-chain acid to a two-necked flask equipped with a stirring device and a condenser in a certain proportion, adding an appropriate amount of Sn(Oct)2 (1%wt) as a catalyst, and heating the esterification reaction to 190°C for 3 hours under nitrogen protection until no more water is distilled out.

[0011] Preferably, step (2) specifically includes: adding the diol with long carbon side chains obtained in step (1) into a three-necked reaction vessel, setting up a vacuum device, adjusting the temperature of the oil bath to 120°C, dehydrating under a vacuum of -0.095 MPa for 1.5 h, cooling to 90°C, adding diisocyanate and polyether diol into a three-necked flask, cooling the sample to 85°C after dissolving, and passing nitrogen gas through to react for about 1.5 h to obtain a small molecule prepolymer.

[0012] Preferably, step (3) specifically includes: adding the chain extender to the small molecule prepolymer obtained in step (2), stirring quickly and evenly, pouring the reaction solution into a preheated polytetrafluoroethylene mold, and then placing it in a flat vulcanizing machine. First, preheat and pressurize it at 140°C to 220°C for 10 minutes, and then cold press it for 5 minutes to obtain the long carbon chain modified high melt strength TPU material.

[0013] Preferably, step (4) specifically includes: placing an appropriate amount of long-chain modified high melt strength TPU material obtained in step (3) in a constant temperature oven, setting the temperature to 80°C, drying for 4 hours, and then packaging it in a sealed bag for later use; adding carbon dioxide, TPU material and foam stabilizer to a high-pressure reactor and stirring evenly; after ensuring airtightness, controlling the temperature and pressure inside the reactor through a control box and a gas booster pump; after meeting the required saturation time and foaming temperature and pressure, rapidly depressurizing to atmospheric pressure within 1 second to obtain a long-chain modified high melt strength TPU foaming material.

[0014] The above-described solution of the present invention has at least the following beneficial effects: (1) The long-chain modified high melt strength TPU foaming material of the present invention is synthesized from pentaerythritol, long-chain acid, diisocyanate, polyether diol, chain extender, catalyst and foam stabilizer as raw materials. The shortcoming of commercially available TPU foaming materials is that the molecular chains do not form chemical cross-links, so the heat resistance and melt strength of TPU foaming materials are poor. During the foaming process, when the cell walls grow in the cell, there is not enough deformation space, and the cell walls are prone to breakage. Faced with the problems of low melt strength and difficulty in forming pores in TPU foaming materials, if the degree of chemical cross-linking between TPU molecular chains is greatly increased, the TPU foaming material will not be able to melt and will not meet the foaming conditions. The long-chain modified high melt strength TPU foaming material of the present invention can avoid the above problems. Because the soft segments of TPU are diols with long carbon chains, the physical entanglement between molecular chains increases after TPU synthesis, enhancing the physical cross-linking effect and significantly improving the viscoelasticity of the TPU melt. This provides sufficient deformation space for the cell walls during cell growth, while also strengthening the cell walls, hindering gas diffusion within the cells, reducing the gas diffusion rate within the cells, improving the shrinkage resistance of the TPU material, and significantly improving the melt strength of the TPU foam material. This solves the problems of low melt strength and difficulty in cell formation during the foaming process of TPU foam materials.

[0015] (2) The preparation method of the long carbon chain modified high melt strength TPU foaming material of the present invention includes the following steps: taking pentaerythritol and long carbon chain acid by weight, first performing esterification reaction to obtain a diol with long carbon chain side chain, then mixing the obtained diol with long carbon chain side chain, diisocyanate and polyether diol evenly, performing prepolymerization reaction to obtain a small molecule prepolymer, adding chain extender and foam stabilizer to the small molecule prepolymer, reacting to obtain long carbon chain modified high melt strength TPU material, passing it and carbon dioxide into a high pressure reactor, adjusting to a suitable temperature, pressure and saturation time, then quickly depressurizing to atmospheric pressure, reacting to obtain long carbon chain modified high melt strength TPU foaming material.

[0016] (3) The preparation method of the long carbon chain modified high melt strength TPU foaming material of the present invention is simple and solves the problem of the harsh requirements for the preparation of high melt strength TPU foaming material in the prior art, and has good application prospects. Detailed Implementation

[0017] Exemplary embodiments of this disclosure will now be described in more detail. While exemplary embodiments of this disclosure have been shown, it should be understood that this disclosure may be implemented in various forms and should not be limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of this disclosure to those skilled in the art.

[0018] Unless otherwise specified in the embodiments of this invention, the conditions shall be performed under conventional conditions or conditions recommended by the manufacturer. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products. The following only provides some of the reagents used in the embodiments of this invention; different manufacturers and models of raw materials do not affect the implementation of the technical solution or the achievement of the technical effect of this invention.

[0019]

[0020] Example 1 This embodiment is synthesized from the following raw materials in parts by weight: 100 parts by weight of diisocyanate, 6 parts by weight of pentaerythritol, 12 parts by weight of long-chain acid, 104 parts by weight of polyether diol, 2 parts by weight of chain extender, 3 parts by weight of catalyst, and 2 parts by weight of foam stabilizer.

[0021] Wherein, the long carbon chain is octanoic acid; the diisocyanate is p-phenyl diisocyanate; the polyether diol is polyether N210; the chain extender is 1,4-butanediol; the catalyst is dibutyltin dilaurate; and the foam stabilizer is a copolymer of polyether and silicone oil.

[0022] The long carbon chain modified small molecule beads have the structure shown in formula (I):

[0023] (I) Where n is an integer greater than or equal to 8.

[0024] The preparation method of the long carbon chain modified high melt strength TPU foaming material described in this embodiment includes the following steps: (1) Reaction of pentaerythritol with a long-chain acid yields a diol with a long-chain side chain, as shown in the following reaction formula: Where n is an integer greater than or equal to 8.

[0025] (2) The diols and diisocyanates with long carbon side chains obtained in step (1) are mixed evenly with polyether diols and reacted to obtain small molecule prepolymers;

[0026] Where n is an integer greater than or equal to 8.

[0027] (3) Add chain extender and foam stabilizer to the small molecule prepolymer obtained in step (2) and react to obtain long carbon chain modified high melt strength TPU material.

[0028] (4) The long carbon chain modified high melt strength TPU material obtained in step (3) is introduced into a high pressure reactor with carbon dioxide. After adjusting to a suitable temperature, pressure and saturation time, the pressure is quickly released to atmospheric pressure to obtain a long carbon chain modified high melt strength TPU foam material.

[0029] The long-chain modified high melt strength TPU foaming material described in this embodiment specifically includes the following steps: (1) Add pentaerythritol and long-chain acid to a two-necked flask equipped with a stirring device and a condenser in a certain proportion, add an appropriate amount of catalyst, and heat the esterification reaction to 190°C for 3 hours under nitrogen protection until no more water is distilled out.

[0030] (2) Add the long carbon chain diol obtained in step (1) into a three-necked reaction vessel, set up a vacuum device, adjust the oil bath temperature to 120°C, dehydrate for 1.5 h under vacuum of -0.095 MPa, cool to 90°C, add diisocyanate and polyether diol into a three-necked flask, cool to 85°C after the sample dissolves, and purge with nitrogen for about 1.5 h to obtain a small molecule prepolymer.

[0031] (3) Add the chain extender and foam stabilizer to the small molecule prepolymer obtained in step (2), stir quickly and evenly, pour the reaction solution into the preheated polytetrafluoroethylene mold, and then place it in a flat vulcanizing machine. First, preheat and press for 10 minutes at 140°C to 220°C, and then cold press for 5 minutes to obtain the long carbon chain modified high melt strength TPU material.

[0032] (4) Place an appropriate amount of the long-chain modified high melt strength TPU material obtained in step (3) in a constant temperature oven, set the temperature to 80℃, dry for 4 hours, and then package it in a sealed bag for later use. Add TPU material to the high-pressure reactor. After ensuring airtightness, control the temperature and pressure inside the reactor through the control box and gas booster pump. After meeting the required saturation time, foaming temperature, and pressure, quickly depressurize to atmospheric pressure within 1 second to obtain the long-chain modified high melt strength TPU foam material.

[0033] Example 2 The long-chain modified high melt strength TPU foaming material of this embodiment is synthesized from the following raw materials in parts by weight: 100 parts by weight of diisocyanate, 20 parts by weight of pentaerythritol, 41 parts by weight of long-chain acid, 96 parts by weight of polyether diol, 2 parts by weight of chain extender, 4 parts by weight of catalyst, and 2 parts by weight of foam stabilizer.

[0034] In this embodiment, the long carbon chain is octanoic acid; the diisocyanate is p-phenyl diisocyanate; the polyether diol is polyether N210; the chain extender is 1,4-butanediol; the catalyst is dibutyltin dilaurate; and the foam stabilizer is a copolymer of polyether and silicone oil. The subsequent preparation process is the same as in Example 1.

[0035] Example 3 The long-chain modified high melt strength TPU foaming material of this embodiment is synthesized from the following raw materials in parts by weight: 100 parts by weight of diisocyanate, 24 parts by weight of pentaerythritol, 48 parts by weight of long-chain acid, 88 parts by weight of polyether diol, 3 parts by weight of chain extender, 3 parts by weight of catalyst, and 2 parts by weight of foam stabilizer.

[0036] In this embodiment, the long carbon chain is octanoic acid; the diisocyanate is p-phenyl diisocyanate; the polyether diol is polyether N210; the chain extender is 1,4-butanediol; the catalyst is dibutyltin dilaurate; and the foam stabilizer is a copolymer of polyether and silicone oil. The subsequent preparation process is the same as in Example 1.

[0037] Example 4 The long-chain modified high melt strength TPU foaming material of this embodiment is synthesized from the following raw materials in parts by weight: 100 parts by weight of diisocyanate, 9 parts by weight of pentaerythritol, 23 parts by weight of long-chain acid, 98 parts by weight of polyether diol, 3 parts by weight of chain extender, 4 parts by weight of catalyst, and 2 parts by weight of foam stabilizer.

[0038] The long-chain acid is lauric acid; the diisocyanate is p-phenyl diisocyanate; the polyether diol is polyether N210; the chain extender is 1,4-butanediol; the catalyst is dibutyltin dilaurate; and the foam stabilizer is a copolymer of polyether and silicone oil. The subsequent preparation process is the same as in Example 1.

[0039] Comparative Example 1 The comparative example is prepared using the same method as Example 1, except that it does not include pentaerythritol and long-chain acids, and step (1) is omitted, i.e., the diisocyanate is directly reacted with the polyether diol. The amount of the polyether diol is replaced by 107 parts by weight instead of 104 parts by weight.

[0040] Effect Comparison To verify the effectiveness of the long-carbon-chain modified high melt strength TPU foaming material described in this invention, the following experiments were conducted: The long-chain modified high melt strength TPU foam materials prepared in Comparative Example 1 and Examples 1-4 were used as test samples. After standing for 24 hours, their melt strength was tested. The specific steps are as follows: Melt strength tests were performed on the samples using a Gottfert Rheotech N71.97 melt tester (Gottfert GmbH, Germany). The polymer melt was extruded from a capillary tube, and the melt stream moved downwards under the traction of a pair of rollers. Since the rollers were directly connected to the force measurement system, the melt tensile strength of each sample on the traction rollers could be directly measured. The test temperature was 190 °C, and the roller rotation speed was 6 mm / s. 2 The acceleration continuously increases. The long-chain modified high melt strength TPU foaming materials prepared in Comparative Example 1 and Examples 1-4 were used to prepare ETPU beads via pressure foaming. The specific steps are as follows: TPU material was added to a high-pressure reactor. The temperature inside the reactor was controlled at 150°C and the pressure at 10 MPa using a control box and a gas booster pump. The saturation time was 3 hours. The pressure was rapidly released to atmospheric pressure within 1 second to obtain long-chain modified high melt strength TPU foaming beads.

[0041] The melt strength test results of the samples are as follows:

[0042] Example 4 strength is 9, Example 3 is 8, Example 2 is 6, Example 1 is 4, and the comparative example is 2.

Claims

1. A long-chain modified high melt strength TPU foaming material, characterized in that, It is synthesized from pentaerythritol, long-chain acid, diisocyanate, polyether diol, chain extender, catalyst and foam stabilizer as raw materials; The preparation method of the long-chain modified high melt strength TPU foaming material includes the following steps: (1) Take pentaerythritol and react it with a long-chain acid to obtain a diol with a long-chain side chain; The long-chain acid is one or more of octanoic acid, lauric acid, palmitic acid, ligninic acid, and beeswaxic acid; (2) Mix the diol with long carbon chain side chain, diisocyanate and polyether diol obtained in step (1) evenly and react to obtain small molecule prepolymer; (3) Add chain extender and foam stabilizer to the small molecule prepolymer obtained in step (2) and react to obtain long carbon chain modified high melt strength TPU material; (4) The long carbon chain modified high melt strength TPU material obtained in step (3) is introduced into a high pressure reactor along with a foam stabilizer and carbon dioxide. After adjusting to a suitable temperature, pressure and saturation time, the pressure is quickly released to atmospheric pressure to obtain a long carbon chain modified high melt strength TPU foaming material.

2. The long-chain modified high melt strength TPU foaming material according to claim 1, characterized in that, It is synthesized from the following raw materials in parts by weight: Pentaerythritol 6-32 parts by weight, long-chain acid 12-64 parts by weight, diisocyanate 100 parts by weight, polyether diol 60-110 parts by weight, chain extender 2-3 parts by weight, catalyst 3-5 parts by weight, foam stabilizer 2-4 parts by weight.

3. The long-chain modified high melt strength TPU foaming material according to claim 1, characterized in that, Optionally, the diisocyanate is one of diphenylmethane diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, p-phenyl diisocyanate, 1,5-naphthalene diisocyanate, and p-phenyl dimethylene diisocyanate. Optionally, the polyether diol is one of polyether N-210, polyether N-220, and polyether N-240; Optionally, the chain extender is one of 1,4-butanediol, 1,4-cyclohexanediol, and p-phenyldimethyldiol; Optionally, the catalyst is one or more of the following: dimethylaminoethyl ether, pentamethyldiethylenetriamine, dimethylcyclohexylamine, dibutyltin dilaurate, organobismuth, and triazine trimerizing catalyst; Optionally, the foam stabilizer is a copolymer of polyether and silicone oil.

4. The long-chain modified high melt strength TPU foaming material according to claim 1, characterized in that, In step (1), the reaction temperature is 180-190℃ and the reaction time is 2-3h; Optionally, in step (2), the reaction temperature is 85-120℃ and the reaction time is 3-4h; Optionally, in step (3), the reaction temperature is 140-220℃ and the reaction time is 0.1-1h; Optionally, in step (4), the reaction temperature is 70-80℃ and the reaction time is 4-5h.

5. The long-chain modified high melt strength TPU foaming material according to claim 1, characterized in that, Step (1) specifically includes: adding pentaerythritol and long-chain acid to a two-necked flask equipped with a stirring device and a condenser in a certain proportion, adding an appropriate amount of catalyst, and heating the esterification reaction to 180-190℃ for 2-3 hours under nitrogen protection until no more water is distilled out.

6. The long-chain modified high melt strength TPU foaming material according to claim 1, characterized in that, In step (2), the diol with long carbon side chains obtained in step (1) is added to a three-necked reaction vessel, a vacuum device is set up, the oil bath temperature is adjusted to 120°C, and dehydrated for 1.5 h under a vacuum of -0.095 MPa. After cooling to 90°C, diisocyanate and polyether diol are added to the three-necked flask. After the sample is dissolved, the temperature is lowered to 85°C, and nitrogen is introduced to react for about 1.5 h. The reaction yields a small molecule prepolymer.

7. The long-chain modified high melt strength TPU foaming material according to claim 1, characterized in that, Step (3) includes: adding the chain extender and foam stabilizer to the small molecule prepolymer obtained in step (2), stirring quickly and evenly, pouring the reaction solution into a preheated polytetrafluoroethylene mold, and then placing it in a flat vulcanizing machine. First, preheat and pressurize it at 140°C to 220°C for 10 minutes, and then cold press it for 5 minutes to obtain the long carbon chain modified high melt strength TPU material.

8. The long-chain modified high melt strength TPU foaming material according to claim 4, characterized in that, Step (4) specifically includes: crushing an appropriate amount of long carbon chain modified high melt strength TPU material obtained in step (3) into granules, placing them in a constant temperature oven, setting the temperature to 80℃, drying for 4 hours, and then packaging them in a sealed bag for later use; adding TPU material to a high pressure reactor, controlling the temperature and pressure inside the reactor through a control box and a gas booster pump; after meeting the required saturation time and foaming temperature and pressure, rapidly depressurizing to atmospheric pressure within 1 second to obtain long carbon chain modified high melt strength TPU foam beads.

9. The application of the long carbon chain modified high melt strength TPU foaming material according to any one of claims 1-3 in the field of polymer materials.

Citation Information

Patent Citations

  • Long-chain branched polylactic resin and preparation method and application thereof

    CN102675577A

  • Low-hardness polyurethane elastomer material

    CN107501510A