Eutectic solvent for recycling lithium and cobalt in lithium battery cathode material and recycling method
By using a eutectic solvent consisting of polyethylene glycol dicarboxylic acid and either Girard reagent T or Girard reagent P, the problems of equipment corrosion and pollution in traditional recycling methods have been solved, achieving efficient recovery of lithium and cobalt and improving safety and recovery rate.
Patent Information
- Application Number
- CN202410113359.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-26
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-01-26
AI Technical Summary
Traditional methods for recycling lithium and cobalt from lithium battery cathode materials suffer from problems such as high acidity corroding equipment, release of toxic gaseous pollutants, and difficulty in treating waste acid, resulting in insufficient environmental friendliness and safety.
A eutectic solvent consisting of polyethylene glycol dicarboxylic acid as a hydrogen bond donor and either Girard reagent T or Girard reagent P as a hydrogen bond acceptor was used to extract lithium and cobalt at a low temperature and for a short time by stirring. The solid products were then separated by water-based solvent and calcined.
This technology enables efficient recovery of lithium and cobalt from lithium-ion battery cathode materials at lower temperatures and in shorter timeframes. It is simple to operate, reduces environmental pollution, and improves safety and recovery rate.
Smart Images

Figure HDA0004684189770000011
Abstract
Description
Technical Field
[0001] This invention belongs to the field of waste lithium battery recycling technology, specifically relating to a low eutectic solvent for recycling lithium and cobalt in lithium battery cathode materials and a recycling method. Background Technology
[0002] Lithium-ion batteries are widely used in electric vehicles and mobile electronic devices. As lithium-ion batteries are used, their charge / discharge performance gradually declines until they are no longer usable, with a typical lifespan of 3-5 years. Used lithium-ion batteries are considered hazardous waste and cannot be directly discarded; they must undergo proper treatment. Furthermore, the cathode materials in lithium-ion batteries (such as LiCoO2) contain metallic lithium (Li) and metallic cobalt (Co), which have high commercial value. Therefore, recycling the metallic Li and Co from the cathode materials of used lithium-ion batteries not only achieves waste reuse but also generates considerable economic benefits.
[0003] Traditional methods for recycling spent lithium-ion battery cathode materials employ hydrometallurgy, using aqueous solutions of inorganic acids such as H₂SO₄, HCl, and HNO₃ as leaching agents. The strong acidity of these acids dissolves the spent lithium-ion battery cathode materials, demonstrating a certain recycling efficiency. However, this process uses high concentrations of acid, which can corrode equipment and release SO₃, HCl, and NO₃. x The leaching process produces toxic gaseous pollutants, and the resulting waste acid is difficult to treat, posing potential hazards to human health and the environment. Therefore, traditional recycling methods have problems in terms of both environmental friendliness and safety. Summary of the Invention
[0004] The technical problem to be solved by the present invention is to address the shortcomings of the existing technology by providing a eutectic solvent and a method for recovering lithium and cobalt from lithium battery cathode materials. This eutectic solvent can achieve efficient extraction and recovery of lithium and cobalt from lithium battery cathode materials at a lower temperature and in a shorter time.
[0005] To address the technical problem proposed in this invention, this invention provides a eutectic solvent for recovering lithium and cobalt from lithium-ion battery cathode materials. The eutectic solvent is composed of a hydrogen bond donor and a hydrogen bond acceptor, wherein the hydrogen bond donor is polyethylene glycol dicarboxylic acid, and the hydrogen bond acceptor is Girard's reagent T(C5H2O). 14 ClN3O) or Girard's reagent P(C7H) 10 ClN3O).
[0006] In the above scheme, the average molecular weight of the polyethylene glycol dicarboxylic acid is 250-600.
[0007] In the above scheme, the molar ratio of the hydrogen bond donor to the hydrogen bond acceptor is 1:(2 to 2.2).
[0008] In the above scheme, the hydrogen bond donor and hydrogen bond acceptor can be mixed to obtain a eutectic solvent, and the mixing temperature is 70-100℃.
[0009] In the above scheme, the stirring rate when mixing the hydrogen bond donor and the hydrogen bond acceptor is 150-300 rpm and the stirring time is 0.5-2 h.
[0010] The present invention also provides a method for recovering lithium and cobalt from lithium battery cathode materials using the above-mentioned eutectic solvent, comprising the following steps:
[0011] 1) The lithium battery cathode material is added to a eutectic solvent and reacted by heating under stirring conditions;
[0012] 2) After the reaction is complete, allow the mixture to cool naturally. During the cooling process, add water to the reactants and stir to dissolve them. Then, centrifuge to obtain a supernatant containing lithium and cobalt.
[0013] In the above scheme, the lithium battery cathode material is lithium cobalt oxide cathode material.
[0014] In the above scheme, the lithium battery cathode material is in powder form with a particle size ≤10μm.
[0015] In the above scheme, the mass ratio of the lithium battery cathode material to the volume ratio of the eutectic solvent is 1g:(20-50)mL.
[0016] In the above scheme, the stirring rate in step 1) is 150-300 rpm.
[0017] In the above scheme, the reaction temperature in step 1) is 70-100℃ and the reaction time is 2-4h.
[0018] In the above scheme, water is added when the reactants are cooled to 60-70°C in step 2).
[0019] In the above scheme, the stirring rate in step 2) is 150-300 rpm and the stirring time is 5-10 min.
[0020] In the above scheme, the volume ratio of water to eutectic solvent is (2-4):1.
[0021] The above scheme also includes step 3), which involves drying the supernatant containing lithium and cobalt and then calcining it to obtain a solid product containing lithium and cobalt.
[0022] Furthermore, the drying is carried out in an air atmosphere, the drying temperature is 100-120℃, and the drying time is 0.5-1h.
[0023] Furthermore, the calcination is carried out in an air atmosphere at a temperature of 500–700°C for 1–2 hours.
[0024] In the above scheme, the eutectic solvent has a lithium recovery rate of ≥88% and a cobalt recovery rate of ≥88% in the lithium battery cathode material.
[0025] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0026] 1) The eutectic solvent of this invention uses polyethylene glycol dicarboxylic acid (PEG-DICA) as a hydrogen bond donor. PEG-DICA has the ability to react with lithium cobalt oxide. The oxygen on its carboxyl group and the oxygen adjacent to the carboxyl group can work together to extract lithium cobalt. However, high temperature conditions are required, reaching 150°C for optimal extraction. Therefore, Girard's reagent T or Girard's reagent P is chosen as the hydrogen bond acceptor. Both Girard's reagent T and Girard's reagent P have structures that readily form hydrogen bonds but do not readily form intermolecular hydrogen bonds with molecules identical to themselves. They can efficiently form a eutectic solvent with PEG-DICA. The active hydrogen in this solvent can easily replace lithium in lithium cobalt oxide, causing lithium ions to escape from the layered structure and promoting the collapse of the crystal structure. As the crystal structure collapses, trivalent cobalt ions are rapidly reduced to divalent cobalt ions by the solvent, and then react with Cl... - Ions form [CoCl4] 2- This promotes the reaction, improves extraction efficiency, and significantly reduces temperature requirements, enabling efficient extraction and recovery of lithium and cobalt from lithium battery cathode materials at lower temperatures and in shorter timeframes.
[0027] 2) This invention uses a eutectic solvent to recover lithium and cobalt from the positive electrode material of lithium batteries. The operation is simple and the extraction process only requires stirring. As lithium and cobalt ions gradually enter the eutectic system, the system gradually becomes viscous, which presents a technical challenge of how to separate the reactants from the unreacted substances. Therefore, water is used as a co-solvent to dissolve and separate the eutectic solvent at a certain temperature to obtain a supernatant containing lithium and cobalt. This supernatant can be dried and calcined to obtain a solid product containing lithium and cobalt. Attached Figure Description
[0028] Figure 1 This is a process state diagram of the recovery of lithium and cobalt from lithium battery cathode materials using a eutectic solvent in Embodiment 1 of the present invention. Detailed Implementation
[0029] To better understand the present invention, the following embodiments further illustrate the content of the present invention, but the content of the present invention is not limited to the following embodiments.
[0030] In the following embodiments, the lithium battery cathode material used is waste lithium cobalt oxide cathode material, which is in powder form with a particle size of 1-10 μm.
[0031] Example 1
[0032] In this embodiment, the eutectic solvent is composed of polyethylene glycol dicarboxylic acid with an average molecular weight of 250 and Gerard's reagent T. The eutectic solvent is prepared by mixing polyethylene glycol dicarboxylic acid and Gerard's reagent T at a molar ratio of 1:2 and stirring at 270 rpm for 1 hour at 80°C.
[0033] The recovery of lithium and cobalt from lithium-ion battery cathode materials using the aforementioned eutectic solvent includes the following steps:
[0034] 1) Add 1g of lithium battery cathode material to 20mL of eutectic solvent, and react at 100℃ for 4h under stirring at 270rpm.
[0035] 2) Allow the reactants to cool naturally to 70°C. Add 60 mL of water and stir at 270 rpm for 5 min to dissolve. Then centrifuge to obtain a supernatant containing lithium and cobalt.
[0036] 3) Place the supernatant containing lithium and cobalt in an air atmosphere, dry it at 100°C for 0.5 h, and then calcine it at 500°C for 2 h to obtain a solid product containing lithium and cobalt.
[0037] Example 2
[0038] In this embodiment, the eutectic solvent is composed of polyethylene glycol dicarboxylic acid with an average molecular weight of 250 and Gillart reagent T. The eutectic solvent is prepared by mixing polyethylene glycol dicarboxylic acid and Gillart reagent T at a molar ratio of 1:2 and stirring at 240 rpm for 2 hours at 100°C.
[0039] The recovery of lithium and cobalt from lithium-ion battery cathode materials using the aforementioned eutectic solvent includes the following steps:
[0040] 1) Add 1g of lithium battery cathode material to 30mL of eutectic solvent, and react at 90℃ for 3h under stirring at 240rpm.
[0041] 2) Allow the reactants to cool naturally to 70°C. Add 60 mL of water and stir at 240 rpm for 5 min to dissolve. Then centrifuge to obtain a supernatant containing lithium and cobalt.
[0042] 3) Place the supernatant containing lithium and cobalt in an air atmosphere, dry it at 110°C for 1 hour, and then calcine it at 550°C for 1.5 hours to obtain a solid product containing lithium and cobalt.
[0043] Example 3
[0044] In this embodiment, the eutectic solvent is composed of polyethylene glycol dicarboxylic acid with an average molecular weight of 250 and Girard reagent P. The eutectic solvent is prepared by mixing polyethylene glycol dicarboxylic acid and Girard reagent P at a molar ratio of 1:2 and stirring at 210 rpm for 2 hours at 100°C.
[0045] The recovery of lithium and cobalt from lithium-ion battery cathode materials using the aforementioned eutectic solvent includes the following steps:
[0046] 1) Add 1g of lithium battery cathode material to 40mL of eutectic solvent, and react at 90℃ for 3h under stirring at 210rpm.
[0047] 2) Natural cooling: When the reactants are cooled to 65°C, add 160 mL of water and stir at 210 rpm for 5 min to dissolve. Then centrifuge to obtain a supernatant containing lithium and cobalt.
[0048] 3) Place the supernatant containing lithium and cobalt in an air atmosphere, dry it at 120°C for 0.5 h, and then calcine it at 600°C for 1 h to obtain a solid product containing lithium and cobalt.
[0049] Example 4
[0050] In this embodiment, the eutectic solvent is composed of polyethylene glycol dicarboxylic acid with an average molecular weight of 600 and Gerard's reagent T. The eutectic solvent is prepared by mixing polyethylene glycol dicarboxylic acid and Gerard's reagent T at a molar ratio of 1:2.2 and stirring at 270 rpm for 2 hours at 100°C.
[0051] The recovery of lithium and cobalt from lithium-ion battery cathode materials using the aforementioned eutectic solvent includes the following steps:
[0052] 1) Add 1g of lithium battery cathode material to 50mL of eutectic solvent, and react at 100℃ for 4h under stirring at 270rpm.
[0053] 2) Natural cooling: When the reactants are cooled to 70°C, add 150 mL of water and stir at 270 rpm for 10 min to dissolve. Then centrifuge to obtain the supernatant containing lithium and cobalt.
[0054] 3) Place the supernatant containing lithium and cobalt in an air atmosphere, dry it at 110°C for 1 hour, and then calcine it at 650°C for 1.5 hours to obtain a solid product containing lithium and cobalt.
[0055] Example 5
[0056] In this embodiment, the eutectic solvent is composed of polyethylene glycol dicarboxylic acid with an average molecular weight of 600 and Girard reagent P. The eutectic solvent is prepared by mixing polyethylene glycol dicarboxylic acid and Girard reagent P at a molar ratio of 1:2.1 and stirring at 180 rpm for 0.5 h at 80 °C.
[0057] The recovery of lithium and cobalt from lithium-ion battery cathode materials using the aforementioned eutectic solvent includes the following steps:
[0058] 1) Add 1g of lithium battery cathode material to 20mL of eutectic solvent, and react at 80℃ for 2h under stirring at 180rpm.
[0059] 2) Allow the reactants to cool naturally to 60°C. Add 40 mL of water and stir at 180 rpm for 10 min to dissolve. Then centrifuge to obtain a supernatant containing lithium and cobalt.
[0060] 3) Place the supernatant containing lithium and cobalt in an air atmosphere, dry it at 100°C for 0.75 h, and then calcine it at 700°C for 2 h to obtain a solid product containing lithium and cobalt.
[0061] Comparative Example 1
[0062] The only difference between Comparative Example 1 and Example 1 is that Gerard's reagent T is not added.
[0063] Comparative Example 2
[0064] The only difference between Comparative Example 2 and Example 1 is that the Gerard reagent T is replaced with L-carnitine.
[0065] Comparative Example 3
[0066] The only difference between Comparative Example 3 and Example 1 is that Gillard reagent T is replaced with meldonium.
[0067] Comparative Example 4
[0068] The only difference between Comparative Example 4 and Example 1 is that Gilard's reagent T is replaced with choline chloride.
[0069] The recovery rates of each embodiment and comparative example were tested. The recovery rate could be tested by comparing the lithium cobalt content in the supernatant with the lithium cobalt content in the lithium battery cathode material, or by comparing the lithium cobalt content in the solid product with the lithium cobalt content in the lithium battery cathode material. The results obtained by the two methods were consistent, and the results are shown in the table below.
[0070] Table 1
[0071] serial number Lithium recovery rate Cobalt recovery rate Example 1 96.76% 97.88% Example 2 96.47% 97.15% Example 3 92.31% 93.55% Example 4 92.57% 99.52% Example 5 88.31% 88.22% Comparative Example 1 55.30% 39.60% Comparative Example 2 8.13% 7.14% Comparative Example 3 9.33% 7.48% Comparative Example 4 32.57% 34.02%
[0072] As can be seen from Table 1, the eutectic solvent of the present invention can achieve efficient extraction and recovery of lithium and cobalt in lithium battery cathode materials at a lower temperature and in a shorter time. However, when polyethylene glycol dicarboxylic acid is used alone, the extraction efficiency of lithium and cobalt is low under low temperature conditions. When polyethylene glycol dicarboxylic acid is combined with other hydrogen bond acceptors, the expected effect cannot be achieved.
[0073] The above embodiments are merely examples for clear illustration and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations, and any obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A eutectic solvent for recovering lithium and cobalt from lithium-ion battery cathode materials, comprising a hydrogen bond donor and a hydrogen bond acceptor, characterized in that, The hydrogen bond donor is polyethylene glycol dicarboxylic acid with an average molecular weight of 250-600, and the hydrogen bond acceptor is Girard reagent T or Girard reagent P. The molar ratio of hydrogen bond donor to hydrogen bond acceptor is 1:(2-2.2).
2. The eutectic solvent for recovering lithium and cobalt in lithium battery cathode materials according to claim 1, characterized in that, The hydrogen bond donor and hydrogen bond acceptor are mixed to obtain a eutectic solvent, and the mixing temperature is 70~100℃.
3. A method for recovering lithium and cobalt from lithium battery cathode materials using the eutectic solvent according to any one of claims 1 to 2, characterized in that, Includes the following steps: 1) The lithium battery cathode material is added to a eutectic solvent and the reaction is carried out under stirring and heating. 2) After the reaction is complete, allow the mixture to cool naturally. During the cooling process, add water to the reactants and stir to dissolve them. Then, centrifuge to obtain a supernatant containing lithium and cobalt.
4. The method for recovering lithium and cobalt from lithium battery cathode materials according to claim 3, characterized in that, The lithium battery cathode material is a lithium cobalt oxide cathode material, and the mass ratio of the lithium battery cathode material to the volume ratio of the eutectic solvent is 1g:(20~50)mL.
5. The method for recovering lithium and cobalt from lithium battery cathode materials according to claim 3, characterized in that, The reaction temperature in step 1) is 70~100℃ and the reaction time is 2~4h.
6. The method for recovering lithium and cobalt from lithium battery cathode materials according to claim 3, characterized in that, In step 2), water is added when the reactants are cooled to 60-70°C, and the volume ratio of water to eutectic solvent is (2-4):
1.
7. The method for recovering lithium and cobalt from lithium battery cathode materials according to claim 3, characterized in that, It also includes step 3), which involves drying the supernatant containing lithium and cobalt and then calcining it to obtain a solid product containing lithium and cobalt.
8. The method for recovering lithium and cobalt from lithium battery cathode materials according to claim 7, characterized in that, The drying temperature is 100~120℃, and the drying time is 0.5~1h; the calcination temperature is 500~700℃, and the calcination time is 1~2h.
Citation Information
Patent Citations
Eutectic solvent for fuel extraction and denitrification and use method thereof
CN109181747A
Eutectic solvent and method for extracting and removing oxygen-containing compound in oil product by using eutectic solvent