Process for the production of ferro-niobium alloys from niobium-aluminium scrap

By controlling the order and particle size of adding iron oxide and niobium-aluminum scrap through medium-frequency furnace smelting, the problem of high aluminum content in niobium-aluminum scrap during the production of niobium-iron alloys was solved, achieving efficient production of niobium-iron alloys and improving the yield of niobium and the purity of the alloy.

CN118006951BActive Publication Date: 2026-11-20CNMC NINGXIA ORIENT GRP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410154981.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-04
Publication Date
2026-11-20
Estimated Expiration
2044-02-04

AI Technical Summary

Technical Problem

In existing technologies, the production of niobium-iron alloys from niobium-aluminum scrap results in high aluminum content, high costs, and low niobium yield, making it difficult to utilize effectively. Furthermore, existing methods cannot precisely control the alloy composition.

Method used

The medium-frequency furnace smelting method is adopted. By controlling the order and particle size of adding iron oxide and niobium-aluminum waste, the niobium-aluminum waste is first granulated and mixed with iron oxide powder, and then added to the medium-frequency furnace in batches. The reaction between aluminum and iron oxide is controlled to generate niobium-iron alloy, reduce the aluminum content in the alloy liquid, and improve the niobium yield.

Benefits of technology

It achieved a niobium recovery rate of 99%, the alloy composition met user requirements, reduced production costs, and improved the purity of ferroniobium alloys and the niobium recovery rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004696765680000051
    Figure BDA0004696765680000051
  • Figure BDA0004696765680000061
    Figure BDA0004696765680000061
  • Figure BDA0004696765680000071
    Figure BDA0004696765680000071
Patent Text Reader

Abstract

The method for producing niobium-iron alloy from niobium-aluminum waste material comprises the following steps: ingredient mixing, raw material treatment, adding waste iron, adding calcium oxide, preheating and temperature rising, adding iron oxide, adding niobium-aluminum waste material in batches, and continuously smelting with increased power; by means of the intermediate frequency furnace smelting into molten liquid, the elemental aluminum is removed by using iron oxide, and the obtained elemental iron is put into the alloy liquid, and the niobium is not lost in the whole process, the yield of niobium obtained from the waste material reaches 99%, and the content of niobium and iron in the alloy is effectively controlled, which can fully meet the requirements of users on the content of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of alloy smelting technology, and in particular to a method for producing niobium-iron alloy from niobium-aluminum waste. Background Technology

[0002] Niobium-aluminum recycled materials smelted in electron beam furnaces are treated as waste due to their high aluminum content, making it impossible to fully utilize the niobium.

[0003] Existing methods for producing ferroniobium alloys include the aluminothermic reduction method, which involves reducing niobium oxide and iron oxide. This method requires the separate addition of reducing agents, consumes a large amount of aluminum, and is therefore costly. Other manufacturers recycle niobium-aluminum waste and use the aluminothermic method to produce ferroniobium. However, this requires the addition of nitrate as a heating agent and also necessitates the supplementation of aluminum granules, resulting in high production costs, low niobium yield, and hindering industrialization. Summary of the Invention

[0004] In view of the above deficiencies, the present invention proposes a method for producing niobium-iron alloy from niobium-aluminum waste, characterized by comprising the following steps:

[0005] S1: Weigh the raw materials according to the following weight ratio: niobium aluminum scrap: iron oxide powder: scrap iron: calcium oxide

[0006] = 1:0.2~0.5:0.03~0.4:0.05~0.2;

[0007] S2: Raw material processing: Niobium aluminum waste and iron oxide powder are granulated to 3-10mm and then dried.

[0008] S3: Load the scrap iron and calcium oxide into the medium frequency furnace in sequence;

[0009] S4: Preheat the medium-frequency furnace containing the material with a power of less than 40KW for 10-30 minutes; S5: Melt the preheated material.

[0010] S6: After the material has melted and cleared, add granular iron oxide powder;

[0011] S7: After the iron oxide powder has melted and cleared, increase the heating power of the medium frequency furnace to 60-80KW, and add niobium-aluminum scrap in batches to allow the aluminum in the niobium-aluminum scrap to react with the oxides in the molten metal. After the reaction flame is stable, continue to add the next batch of niobium-aluminum scrap until all scrap is added.

[0012] S8: After the niobium-aluminum scrap is added, increase the smelting power of the medium frequency furnace to 120KW. After the slag liquid is leveled, proceed with slag removal and alloy liquid removal in sequence to obtain niobium-iron alloy.

[0013] In this invention, due to limitations of existing detection methods and means, it is impossible to accurately detect the components in the waste, to separately detect niobium oxide and niobium, and to separately detect aluminum oxide and aluminum. Therefore, by making assumptions, the detected niobium content is set to be entirely elemental niobium (since the source is an electron beam furnace, this treatment volatilizes the elemental aluminum of the niobium-aluminum alloy. This process will at most generate a small amount of aluminum oxide and almost no niobium oxide, so the niobium oxide content is extremely low and can be ignored), and the detected aluminum content is set to be entirely elemental aluminum. The amount of iron oxide added is calculated based on the aluminum content. This method can make the maximum assumption of aluminum reducing iron oxide, so that all elemental aluminum participates in the reduction reaction and is extracted. Even if some aluminum oxide is present, it will enter the slag layer in the form of oxides and will not enter the alloy liquid.

[0014] This invention employs a medium-frequency furnace to melt aluminum into a liquid, using iron oxide to remove elemental aluminum. Simultaneously, the resulting elemental iron enters the alloy liquid, resulting in zero niobium loss throughout the process. The niobium yield from waste reaches 99%, and the niobium and iron content in the alloy is effectively controlled, fully meeting the user's requirements for product content.

[0015] This is completely different from the existing technology of preparing niobium-aluminum alloys using the aluminothermic reduction method. When using the aluminothermic reduction method, the content of elemental aluminum and alumina in the niobium-aluminum scrap cannot be determined, resulting in extremely high aluminum residue in the alloy after the ignition reaction, and the quality is completely uncontrollable. Detailed Implementation

[0016] A method for producing ferroniobium alloy from niobium-aluminum scrap includes the following steps:

[0017] S1: Weigh the raw materials according to the weight ratio: Niobium aluminum waste: Iron oxide powder: Scrap iron: Calcium oxide = 1:0.2~0.5:0.03~0.4:0.05~0.2;

[0018] S2: Raw material processing: Niobium-aluminum waste and iron oxide powder are granulated to 3-10mm and dried at 150℃. In this step, due to the fine particle size of niobium-aluminum waste and iron oxide, there is not only the problem of dust cost during operation, but more importantly, during the process of adding to the medium frequency furnace, this scheme pre-forms an oxide slag layer. When niobium-aluminum waste and iron oxide powder that are too fine are added to the furnace, they will float on the slag layer due to their fine particle size and cannot enter the alloy liquid smoothly. Therefore, by granulation, the particle size is increased and the specific gravity is increased, so that the slag layer is broken and the powder enters the alloy liquid when it is added.

[0019] S3: Load the scrap iron and calcium oxide into the medium frequency furnace in sequence;

[0020] S4: Preheat the medium-frequency furnace containing materials, with a power of less than 40KW, for 10 to 30 minutes;

[0021] S5: Heat up and melt the preheated material;

[0022] S6: After the material has melted and cleared, add granular iron oxide powder;

[0023] S7: After the iron oxide powder has melted and cleared, increase the heating power of the medium frequency furnace to 60-80KW, and add niobium-aluminum scrap in batches, about 15kg per batch, so that the aluminum in the niobium-aluminum scrap reacts with the oxides in the molten metal. After the reaction flame is stable, continue to add the next batch of niobium-aluminum scrap until all the scrap is added. In this step, the main reaction is that the aluminum in the scrap reduces the iron oxide, which not only yields elemental iron, but also reduces the aluminum content in the scrap, thus reducing the aluminum content in the generated niobium-aluminum alloy liquid. Therefore, in order to promote a full and rapid reaction between elemental aluminum and iron oxide, iron oxide is added first in this step. After melting, the iron oxide is already in a high-temperature molten state. When adding niobium-aluminum scrap, since aluminum and niobium are mixed together, and niobium has a high specific gravity, it will quickly sink to the bottom of the furnace after entering the solution, forming part of the alloy liquid. The purpose of this invention is to reduce the aluminum content in the alloy liquid. It is necessary to control the rate at which aluminum sinks with niobium and increase the probability of aluminum reacting with iron oxide. Therefore, this step first melts the iron oxide, making it very active and ready to react. Then, niobium-aluminum scrap is added. The added scrap will pass through the molten iron oxide layer. At this time, aluminum reacts rapidly with the iron oxide it comes into contact with. Adding niobium-aluminum scrap in small batches is also to add aluminum from the scrap in small amounts multiple times, allowing it to fully contact and react with the iron oxide. This allows the aluminum in the scrap to be extracted through the iron oxide, preventing aluminum from entering the alloy liquid with niobium and increasing the aluminum content in the alloy liquid. Furthermore, adding the waste in small, multiple batches allows time and opportunity for the niobium oxide that may be present in the waste to react with the aluminum, enabling the niobium oxide to be reduced to elemental niobium and enter the alloy melt. If the niobium-aluminum waste is added all at once, a large amount of elemental aluminum will be drawn into the furnace bottom and enter the alloy melt, resulting in a persistently high aluminum content in the alloy melt, which would fail to achieve the purpose of this invention. This design differs from the method of "mixing iron oxide and niobium-aluminum scrap together and adding them to the furnace." When added together, the iron oxide needs time to melt before entering the furnace. During this time, aluminum cannot react with the iron oxide and will be drawn into the furnace bottom along with the scrap. This greatly reduces the chance of aluminum reacting with iron oxide, resulting in a high aluminum content in the alloy liquid. Furthermore, although the iron oxide and scrap are mixed and in contact when added together, the aluminum is quickly drawn into the furnace bottom due to the lighter density of iron oxide and the heavier density of the scrap, which mainly consists of niobium. This reduces the chance of aluminum reacting with iron oxide. In addition, although the two are in contact after the mixture is added, the iron oxide has not yet had time to melt. During its melting time, a large amount of aluminum has already entered the furnace bottom. Therefore, in this method, the amount of aluminum reacting with iron oxide is greatly reduced, and a large amount of aluminum has already entered the furnace bottom.

[0024] In this scheme, the addition of iron oxide, after being reduced by aluminum, serves as the source of elemental iron for the formation of the niobium-iron alloy from the alloy liquid. Furthermore, the reduction reaction with aluminum lowers the level of elemental aluminum in the alloy liquid. If elemental iron were added directly in this step, although a niobium-iron alloy could be obtained, the aluminum in the alloy liquid could not be removed, thus failing to achieve the objective of this invention.

[0025] Iron oxide is used in excess. For example, during batching, the weight ratio of iron oxide is greater than 0.5, and can be 0.6 to 0.8. In this scheme, in order to extract as much aluminum as possible from the waste, excess iron oxide is used to react with the waste, allowing the aluminum to react fully and thus reducing the aluminum content in the alloy liquid. At the same time, the excess iron oxide will not affect the alloy liquid because, as an oxide, it will enter the slag layer and be discharged due to its light density, thus not affecting the alloy liquid.

[0026] S8: After the niobium-aluminum scrap is added, increase the smelting power of the medium frequency furnace to 120KW. After the slag liquid is leveled, proceed with slag removal and alloy liquid removal in sequence to obtain niobium-iron alloy.

[0027] Furthermore, the furnace lining of the medium-frequency furnace is an alkaline lining. For example, the lining is made of magnesium oxide or aluminum oxide.

[0028] Furthermore, in step S3, scrap iron is first loaded into the bottom of the induction furnace, and then calcium oxide is loaded into the furnace and spread on top of the scrap iron. The purpose of adding the scrap iron into the furnace first is to form a conductive layer when the induction furnace is energized, thus pre-forming a molten pool. The calcium oxide is spread on the surface of the scrap iron to form an isolation layer, preventing the molten iron from coming into contact with air and forming a large amount of iron oxide, thereby increasing the oxygen content of the alloy liquid.

[0029] Example 1

[0030] The material proportions are based on Table 1, the content of each component is tested as shown in Table 2, and the alloy composition obtained after the method of this invention is shown in Table 3.

[0031]

[0032] After implementation of this embodiment, 252 kg of alloy was obtained. Calculations show that the niobium yield in this embodiment can reach 99.33% ((252*60.75%) / (200*77.06%)). Table 3 shows that the aluminum content decreased from 20.66 in the waste to 1.21, the aluminum impurity removal rate reached 94.14% (1-1.21 / 20.66), the niobium content reached more than 60%, and the balance was iron, which fully meets the specifications of grade 60 niobium-iron alloy.

[0033] Example 2:

[0034] The material proportions are based on Table 4, and the content of each component is tested as shown in Table 5. After the method of this invention, the alloy composition is shown in Table 6.

[0035]

[0036] After implementation of this embodiment, 262 kg of alloy was obtained. Calculation showed that the niobium yield in this embodiment could reach 99.24% ((262*60.13%) / (200*79.37%)). As shown in Table 6, the aluminum content decreased from 20.02 in the waste to 1.01, the aluminum impurity removal rate reached 94.95% (1-1.01 / 20.02), the niobium content reached more than 60%, and the balance was iron, which fully met the specifications of grade 60 niobium-iron alloy.

[0037] Comparative example:

[0038] The raw material preparation and other steps are the same as in Example 1, but steps S6 and S7 are as follows:

[0039] S6: After the material is melted and cleared, mix the iron oxide and niobium aluminum waste evenly, and add them into the furnace in batches, each batch being about 25kg. Increase the heating power of the medium frequency furnace to 60-80KW to allow the aluminum in the niobium aluminum waste to react with the oxides in the molten metal. After the reaction flame is stable, continue to add the next batch of niobium aluminum waste until all the waste is added.

[0040]

[0041] The composition of the alloy liquid was then analyzed as shown in Table 7. The weight of the alloy after the reaction was 247 kg ((247*58.58%) / (200*77.06%)), and the niobium yield was 93.88%. Due to the different ways of adding iron oxide and waste, the aluminum content decreased from 20.66% in the waste to 13.54%. A large amount of aluminum did not have time to participate in the reduction reaction and remained in the alloy liquid. In addition, a large amount of iron oxide was also not reduced, resulting in a low iron content and a high aluminum content in the alloy product. Although the niobium yield was high, the inability to reduce the aluminum content meant that the niobium and iron contents could not be controlled to meet the grade requirements.

[0042] The embodiments of this solution have been described in detail above. However, this solution is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of this patent.

Claims

1. A method for producing niobium-iron alloy from niobium-aluminum waste, characterized in that... Includes the following steps: S1: Weigh the raw materials according to the weight ratio: Niobium aluminum scrap: Iron oxide: Scrap iron: Calcium oxide = 1: 0.2~0.5: 0.03~0.4: 0.05~0.2; S2: Raw material processing: Niobium aluminum waste and iron oxide are granulated to 3-10mm and then dried. S3: Load the scrap iron and calcium oxide into the medium frequency furnace in sequence; S4: Preheat the medium-frequency furnace containing materials with a power of less than 40kW for 10~30min; S5: Heat up and melt the preheated material; S6: After the material has melted and cleared, add granular iron oxide; S7: After the iron oxide powder has melted and cleared, increase the heating power of the medium frequency furnace to 60~80kW, and add niobium-aluminum scrap in batches to allow the aluminum in the niobium-aluminum scrap to react with the oxides in the molten metal. After the reaction flame is stable, continue to add the next batch of niobium-aluminum scrap until all scrap is added. S8: After the niobium-aluminum scrap is added, increase the smelting power of the medium frequency furnace to 120kW. After the slag liquid is leveled, proceed with slag removal and alloy liquid removal in sequence to obtain niobium-iron alloy.

2. The method for producing niobium-iron alloy from niobium-aluminum waste as described in claim 1, characterized in that: The furnace lining of the medium-frequency furnace is an alkaline lining.

3. The method for producing niobium-iron alloy from niobium-aluminum waste as described in claim 1, characterized in that: In step S3, scrap iron is first loaded into the bottom of the medium-frequency furnace, and then calcium oxide is loaded into the furnace and laid on top of the scrap iron.

Citation Information

Patent Citations

  • Preparation method for low-silicon and low-carbon ferroniobium alloy

    CN102605183A

  • Method for casting dealumination of ferrocolumbium

    CN106216645A